Lanthanum-silica sol-gel coatings for protecting metallic materials in museums: approaches to copper, bronze, lead and steel
Abstract
Producción Científica
Full text
coatings Article Lanthanum-Silica Sol-Gel Coatings for Protecting Metallic Materials in Museums: Approaches to Copper, Bronze, Lead and Steel Javier Peña-Poza 1, Fernando Agua 1, Cristina Gil 2, María-Ángeles Villegas 1,* and Manuel García-Heras 1 1Instituto de Historia, CSIC, 28037 Madrid, Spain; javier[email protected] (J.P.-P.); [email protected] (F.A.); [email protected] (M.G.-H.) 2Facultad de Educación, Campus María Zambrano, Universidad de Valladolid, 40005 Segovia, Spain; [email protected] *Correspondence: [email protected]; Tel.: +34-916-022-672 Received: 9 February 2018; Accepted: 10 April 2018; Published: 12 April 2018 Abstract: Museum objects made from metals face the challenge of delaying corrosion in exhibition rooms, showcases and holdings. This study examined some innovative solutions used to protect such items based on sol-gel coatings doped with lanthanum. These coatings were prepared from sols based on TEOS as a precursor. Lanthanum acetate/nitrate was added as a doping agent and corrosion inhibitor. The coatings were deposited upon slabs of copper, bronze, lead and steel, since they are among the most common metals present in museums items. The coatings application was accomplished by immersion-extraction, and the remaining sols were gelled and characterized by Fourier transformed infrared spectroscopy and differential thermal analysis and thermogravimetry. To evaluate the behaviour and resistance of the coatings, tests of accelerated aging were carried out in climatic and Kesternich chambers, as well as under an atmosphere saturated with organic acids and under UV irradiation. The simulated conditions tested were undertaken to approach real conditions inside a conventional museum showcase. The microstructure of the coatings before and after accelerated aging tests was observed through optical and field emission scanning electron microscopies. The results indicated that these coatings can be a useful preventive, conservation avenue to protect copper, bronze and lead items exhibited in museums. Keywords: metals; sol-gel coatings; protection; museum; accelerated ageing; corrosion 1. Introduction Many museum objects and collections are composed of metals and alloys or, at least, have metallic components. As is known, the conservation of metals is critical to guard against the threat of corrosion, degradation and loss of material from the objects [ 1 ]. Since the thermodynamic trend of metal corrosion cannot be avoided, strategies to delay it as far as possible must be enhanced and investigated. Protection procedures, patination techniques and paint systems commonly used for modern metals and metallic objects cannot be applied with any guarantee of safety to historical materials and museum items [ 2 , 3 ]. This is because such items need nonaggressive products, easy application and reversibility as far as possible. Moreover, low-cost protective materials are preferred since museums budgets are limited. Bearing this in mind, few conventional protective procedures are useful for metallic museum items. Among them, sol-gel coatings technology offers a suitable solution [ 4 , 5 ], even though the coatings’ reversibility is only partial. Even so, it is a practical, versatile and inexpensive procedure Coatings 2018,8, 138; doi:10.3390/coatings8040138 www.mdpi.com/journal/coatings
Coatings 2018,8, 138 2 of 15 that can give more advantages than inconveniences for deeply corroded pieces and objects, e.g., archaeological items both unearthed and rescued from the sea waters. Much research has been carried out on sol-gel formulations applied as consolidants for Heritage materials, e.g., different kinds of stones, Portland cement mortars, ceramic tiles, stained glasses, etc. In stones, sol-gel preparations were developed with the aim of reducing cracks inside the stone and/or to modify its hydrophobic character or porous size distribution [ 6 – 9 ]. The results seem to be promising, although some improvements are still needed. For instance, the simple TEOS gel compares less favorably with hydroxyapatite, which when formed at the grains boundaries, improves mechanical properties and yields low variations in porosity and pore size distribution. Moreover, some applications need the simultaneous use of a surfactant to achieve coarse and more uniform pore size to avoid cracks inside the stone [ 8 , 10 ]. For potash-lime-silicate glasses from medieval stained-glass windows, protective coatings based on sol-gel technology have proven to be good enough to guarantee adhesion and resistance against ageing and acids such as HCl, HNO 3 and H 2 SO 4 , even when applied without a thermal densification treatment [ 11 , 12 ]. However, silicon alkoxide/alkylalkoxide hybrid-based gels deposited upon ceramic tiles did not improve the protection provided by Paraloid B-72 (only one coat), even though some polymerization took place and the hydrophobic properties were partially modified by the sol-gel layer [13]. Concerning the usefulness of sol-gel coatings on metallic substrates, they have been widely proved upon steel, aluminum, zinc, magnesium, copper and their alloys [ 14 – 16 ], with the aim of replacing nonenvironmentally friendly Cr 6+ anticorrosive compounds and improving the properties of the metallic substrate. Some strategies have been implemented: hybrid organic-inorganic formulations, multilayered coats, functional purposes, barrier effect, self-repairing mechanism, etc. Sol-gel protective coatings, upon the above-mentioned metals and alloys, also improve upon many industrial applications since these layers are resistant against water, oxidation, abrasion, etc. [17]. Sol-gel coatings doped with lanthanide compounds have been developed and applied for corrosion protection in a wide variety of metallic substrates and alloys [ 18 – 22 ]. These lanthanide compounds improve the sol-gel’s protective benefits [ 23 , 24 ]. Moreover, some investigations have pointed out the capabilities of the combination of lanthanum salts and organic additives, such as benzotriazole and citric acid [25,26]. Corrosion protection measures for metallic museum items have been tested on objects exhibited in both showcases and in exhibition rooms, but these should also be carried out for items conserved in holdings and being transported, e.g., for temporary exhibitions. Therefore, the objectives of the present study were fitted as far as possible to deal with these issues. They can be summarized in three stages: • Design of environmentally friendly sol-gel coatings doped with corrosion inhibitors: lanthanum salts. • Production of these doped sol-gel coatings as a chemically active layer upon copper, bronze, lead and steel substrates. • Study of the coatings’ behaviour under laboratory conditions: thermal, structural, chemical and optical. Two lanthanum salts have been investigated as corrosion inhibitors: lanthanum acetate and lanthanum nitrate. The former is believed to be a compatible compound both with the silica matrix to be formed by hydrolysis and partial polycondensation of silicon tetraethoxide, and with the solvent to be used during the sol preparation (ethanol). The –CH 2 –CH 3 group is present in these three sol components (silica matrix precursor, solvent and dopant), which could improve the gel’s homogeneity in terms of residual organic matter entrapped in the silica network. Moreover, the acetate ions will remain in the gel stage since their thermal decomposition is expected to be at about 450–480 ◦ C (lanthanum oxycarbonate formation) and above 910 ◦ C (lanthanum oxide formation) [ 27 , 28 ]. The latter, lanthanum nitrate, was chosen for its lower release temperature of NO− 3 groups (from ~60 ◦ C) with
Coatings 2018,8, 138 3 of 15 respect to that of –CH 2 –CH 3 groups (~450 ◦ C), which could favour the partial thermal densification of the doped coatings. 2. Materials and Methods The metal substrates used were copper, bronze, lead and steel slabs from 1.0 to 1.5 mm in thickness and at about 20 mm × 30 mm in size. These metallic substrates were selected on the basis of their frequent presence in cultural heritage items, particularly in museums environments. Tables 1–4show, respectively, the results of the chemical analyses carried out for these metallic substrates. Such analyses were undertaken by the respective suppliers. Table 1. Chemical composition of the copper substrates. Substrates Chemical Composition (wt %) Copper Cu Others 99.95 rest Table 2. Chemical composition of the bronze substrates. Substrates Chemical Composition (wt %) (min–max) Bronze Cu Sn Pb Zn Ni Others rest 6–8 5–8 3.5–5.5 0–2 0–1 Table 3. Chemical composition of the lead substrates. Substrates Chemical Composition (wt %) Lead Cu Sn Zn Fe Sb Bi As Ag Cd Pb 0.0319 0.0004 0.0003 0.0007 0.0005 0.0233 0.0002 0.0016 0.0009 rest Table 4. Chemical composition of the steel substrates. Substrates Chemical Composition (wt %) Steel Fe C Mn P S Si Al rest 0.052 0.246 0.019 0.024 0.007 0.051 The sol-gel coatings matrix was obtained from tetraethoxysilane (TEOS) and the active sol-gel dopants were lanthanum acetate and lanthanum nitrate, used separately. Other sol components were absolute ethanol, HNO 3 0.01–0.10 M (up to pH ~3 in the corresponding sols) and distilled water. All the chemicals used were analytical grade reagents. The scheme of Figure 1summarizes the synthesis steps. Figure 1. Scheme of the synthesis steps for obtaining sol-gel coatings and bulk gels.
Coatings 2018,8, 138 4 of 15 The sol-gel formulation was calculated to obtain a theoretical mol composition of 1La 2 O 3· 99SiO 2 (theoretical total densification of the corresponding gel). The sol silica matrix consisted of 1 mol TEOS, 3 mol distilled water, 8 mol absolute ethanol and the necessary volume of HNO 3 to get a sol pH ~ 3. The mixture, once stirred and homogenized, yields a pre-hydrolyzed silica sol to which the active La 3+ -dopant was added (0.02 mol La(CH 3 COO) 3 , (La(Ac) 3 ) or 0.02 mol La(NO 3 ) 3 ). After dissolution of the lanthanum salt and further homogenization of the sols, they were ready to be applied as coatings upon the metallic substrates. For comparison purposes, a pure-silica-undoped sol was also prepared to coat the substrates. The coatings deposition was carried out by dipping, using a home-made device at a constant withdrawal rate of 2 mm s −1 , under controlled environmental conditions (25 ◦ C and 35% relative humidity). The partial thermal densification of the coatings was accomplished in a forced air stove at 60 ◦ C for 72 h. Under such conditions the average coatings’ thickness was about 220 ± 15 nm, as estimated by the interference fringe method from the corresponding UV-Vis transmittance spectra of the coated samples [29]. Apart from the coated metallic samples, common glass slides were additionally coated with the same sols to be used in the optical coatings characterization since, for this purpose, transparent and colourless substrates are needed. Moreover, the remaining sols, once all the coatings were applied, were gelled in a forced air stove at 35 ◦ C for 48 h, and then grounded to a fine powder to be used for the structural and thermal characterization of the gels used to obtain the coatings. The macroscopic aspect of the coatings both on metallic and glass substrates was homogeneous, transparent and colourless. The UV-Vis transmittance spectra of the coated glass samples were recorded with a Shimadzu 3100 double-beam spectrophotometer (Shimadzu Corporation, Kyoto, Japan) equipped with an integrating sphere. Samples were placed behind a 1 mm width slit mask and the spectra were recorded from 200 to 800 nm with 0.5 nm spectral resolution. The thermal behaviour of the coatings (grounded gelled materials) was analyzed by differential thermal analysis (DTA) and thermogravimetric analysis (TGA) using a TA Instruments equipment model Q-600 (Waters Corporation, Milford, MA, USA), with a platinum sample holder under air atmosphere and a heating rate of 10 ◦C min−1up to 700 ◦C. The structural features of the coatings (grounded gelled materials) were investigated by Fourier transformed infrared (FTIR) spectroscopy. The spectra were recorded on the powdered samples diluted in anhydrous KBr (pellets technique) with a spectrometer Perkin Elmer model Spectrum BX (Perkin Elmer Inc., Waltham, MA, USA). The quality of the coatings was checked with conventional optical microscopy (OM), and petrographic microscopy (PM) observations. The optical microscope was a Motic 168 (Motic Microscopy, Hong Kong, China), and the petrographic one was a Kyowa Bio-Pol 2 polarizing light microscope (Kyowa Electronic Instruments Co. Ltd., Tokyo, Japan). Micrographs were recorded with a Moticam 2500 digital camera. The chemical resistance of the coatings was tested by accelerated ageing cycles in a climatic chamber Dycometal model CCK-81 following the ISO-9142 standard [ 30 ], and in a Kesternich chamber Dycometal model VCK-300 under SO 2 atmosphere following the DIN-50018 standard [ 31 ]. Additionally, some other resistance tests were carried out: (i) under an organic acids atmosphere (mixture of HCOOH and CH 3 COOH, since these are the chemicals usually present in the emissions inside museum showcases [ 32 ]); and (ii) optical-ultraviolet (UV) irradiation tests carried out for 21 days, at least. Table 5summarizes the experimental details of the weathering, chemical and optical resistance tests carried out. The microstructural and textural features of the coatings were observed by field emission scanning electron microscopy (FESEM) with a Hitachi S4800FEM equipment (Hitachi, Tokyo, Japan). Local chemical analyses were undertaken by energy dispersive X-ray spectrometry (EDS) with an Oxford X-Max EDS micro-analyzer attached to the microscope.
Coatings 2018,8, 138 5 of 15 Table 5. Experimental details of the weathering and chemical treatments carried out. Treatment Test Equipment Conditions Time Accelerated ageing Climatic chamber Standard ISO-9142 23 ◦C 85% RH 1 day 55 ◦C 28% RH 1 day 23 ◦C 85% RH 3 days 55 ◦C 28% RH 2 days 21 days Accelerated ageing under SO2atmosphere Kesternich corrosion chamber Standard DIN 50018 40 ◦C 100% RH 0.5 L SO 2 8 h closed door 16 h open door 1 cycle Organic acids Desiccator Acetic acid + formic acid (0.01 vol. %) saturated atmosphere 7 days UV irradiation UV lamp 300 W 21 days 3. Results 3.1. Thermal Behaviour Figure 2shows the DTA-TGA diagrams for the undoped pure-silica gel as well as for the gels doped with lanthanum acetate and lanthanum nitrate. Figure 2. DTA and TGA diagrams of some of the samples studied. ( a ) Pure SiO 2 gel; ( b ) La(Ac) 3 doped gel; (c) La(NO3)3doped gel. Table 6summarizes the assignments of the thermal effects detected and the corresponding weight losses for the same gel samples. The thermal effects in lanthanum-doped gels are similar to those of the pure-silica-undoped gel, but some of them overlap. In addition, the incorporation of both lanthanum dopants delays the loss of adsorbed water and alcohols from the sol and the oxidation of the organic precursors. Therefore, a progressive delay of the thermal evolution of the sol-gel matrix takes place.
Coatings 2018,8, 138 6 of 15 Table 6. DTA and TGA assignments of some of the samples studied. Gel Sample DTA TGA T(◦C) Effect T(◦C) Effect 100 SiO2 Blank 73 ENDO Loss adsorbed water and alcohols Room-100 Great loss of water and alcohols 130–220 EXO Organic precursors oxidation 100–300 Great loss due to organic matter release 356 EXO Organic groups decomposition 300–400 522 ENDO Si-OH groups release 500–600 Small loss of chemically bonded water 1La2O3·99SiO2 La(Ac)3 97 ENDO Loss adsorbed water and alcohols Room-135 Great loss of water and alcohols 130–275 EXO Organic precursors oxidation 130–400 Great loss due to organic matter release 350 EXO Organic groups decomposition 500– ENDO Si-OH groups release 500– Progressive loss of chemically bonded water 1La2O3·99SiO2 La(NO3)3 87 ENDO Loss adsorbed water and alcohols Room-140 Great loss of water and alcohols 140–295 EXO Organic precursors oxidation 140–400 Great loss due to organic matter release 300–400 EXO Organic groups decomposition 545 ENDO Si-OH groups release 500– Progressive loss of chemically bonded water TGA diagrams give some additional information on the gels’ behavior (Table 7). At the temperature of partial densification of the coatings (60 ◦ C), the smallest weight loss percentage corresponds to the undoped sample, while in the doped samples it is slightly higher due to the release of adsorbed water additionally associated with the lanthanum salts and perhaps ethanol. The highest weight loss percentage of the La(NO 3 ) 3 doped sample could be explained by the early decomposition of nitrate groups at about 60 ◦ C, which cannot be discarded. Regarding the temperatures at which the 5% weight loss takes place, they decrease from the undoped sample to the doped ones, and the sample doped with La(NO 3 ) 3 shows the lowest value for the same reason stated above: the beginning of the nitrates’ decomposition. Likewise, the final weight loss percentages at the end of the test (~700 ◦ C) increase from the undoped sample to the La(Ac) 3 and to the La(NO 3 ) 3 doped samples, which indicates some more intense densification of doped samples. Temperatures and weight loss percentages at which the maximum weight loss rates occur in each sample indicate that both doped samples behave similarly, while the undoped sample losses the lowest weight at the lowest temperature. This could be explained by the early release of water and ethanol in the pure silica sol-gel network not disturbed by dopants. Table 7. Additional data concerning TGAs of some of the samples studied. Dopant in the Coating Weight Loss at 60 ◦C (%) Temperature at Which 5% Weight Loss Occurs (◦C) Final Weight Loss at 700 ◦C (%) Temperature at Which Maximum Weight Loss Rate Occurs (◦C) Weight Loss at the Maximum Weight Loss Rate (%) None (blank) 3.36 71.67 21.59 65.17 4.03 La(Ac)33.55 70.26 23.88 94.91 9.03 La(NO3)34.06 67.10 25.05 89.94 8.47 3.2. Structural Features FTIR spectra of doped and undoped gel samples are shown in Figure 3. The main vibration assignments are summarized in Table 8. Figure 3. Cont.
Coatings 2018,8, 138 7 of 15 Figure 3. FTIR spectra of some of the samples studied. ( a ) Pure SiO 2 gel; ( b ) La(Ac) 3 doped gel; (c) La(NO3)3doped gel. The bands and assignments of the pure-silica-undoped sample are also present or shifted in the lanthanum-acetate-doped sample, which in addition shows other bands due to La(Ac) 3 . The same occurs for the lanthanum-nitrate-doped sample, which in addition shows other bands due to La(NO 3 ) 3 . However, no bands due to chemical bonds such as La–O–Si were identified [ 33 – 35 ]. This means that La 3+ -ions are physically entrapped in the pores of the silica sol-gel network and, hence, they remain free enough to react during a common corrosion process. Table 8. FTIR assignments of some of the samples studied [36–38]. Gel Sample Wavenumber (cm−1)Assignment Intensity 1Observations 100 SiO2 Blank 465 δSi–O–Si XXXX Siloxane matrix 577; 801 νs Si–O–Si XXX; XXX Siloxane matrix 951 νSi–OH XXX Raw alkoxides 1085 νSi–O; vas Si–O XXXXX Si–OCH3; Si–O–Si 1166 νs C–O XXXXX, x Raw alkoxides 1286 νas C–O XX, x Raw alkoxides 1398; 1450 δCH2X; X Si–R 1637 νC=C XXX Raw alkoxides 2921; 2988 νC–H; νC–H X; X Si–R; –OCH2CH3 3430 νO–H XXXXX Si–OH 1La2O3·99SiO2 La(Ac)3 463 δSi–O–Si ; πCOO– XXX Siloxane matrix; La(Ac)3 564 νLa–O XXX La(Ac)3 800 νs Si–O–Si XXX Siloxane matrix 948 νSi–OH; νC–C XXX Raw alkoxides; La(Ac)3 1083 νSi–O; vas Si–O; νCH3XXXXX Si–OCH3; Si–O–Si; La(Ac)3 1154 νs C–O XXXXX, x Raw alkoxides 1384 δs CH3XXX La(Ac)3 1460 δas CH3X La(Ac)3 1632 νC=C XXX Raw alkoxides 2854; 2925 νs C–H; νC–H X La(Ac)3; Si–R 3433 νO–H XXXXX Si–OH 1La2O3·99SiO2 La(NO3)3 457 δSi–O–Si XXXX Siloxane matrix 565 νLa–O XXX LaO(NO3) 798 νNO3−XXX La(NO3)3 944 νSi–OH XXX Raw alkoxides 1084 νSi–O; vas Si–O XXXXX Si–OCH3; Si–O–Si 1160 νs C–O XXXXX, x Raw alkoxides 1387; 1463 δCH2X; X Si–R 1632 νC=C XXX Raw alkoxides 2850; 2925 νs C–H X Si–R 3429 νO–H XXXXX Si–OH Note: 1XXXXX very intense; XXXX intense; XXX medium; XX low; X very low; x shoulder.
Coatings 2018,8, 138 8 of 15 3.3. Macroscopic Quality After the accelerated ageing treatment in the climatic chamber, all the metallic coated substrates resist well the weathering conditions (up to 55 ◦ C and 85% relative humidity, 21 days). After the treatment in the Kesternich chamber, which simulates a polluted environment (up to 40 ◦ C and 100% relative humidity under SO 2 atmosphere), copper, bronze and lead coated samples do not show deterioration or corrosion signs, while small surface pits appeared in coated steel. The same occurs after treatment under a mixture of organic acids (formic and acetic acids), i.e., only the coated steel samples show deterioration signs and the formation of more or less interconnected pits (Figure 4). Figure 4. MO images of uncoated and coated areas of some of the samples studied after the weathering tests indicated. ( a ) Copper, x14, La(NO 3 ) 3 doped coating, Kesternich Chamber; ( b ) Bronze, x14, La(Ac) 3 doped coating, organic acids treatment; ( c ) Lead, x14, La(NO 3 ) 3 doped coating, Kesternich Chamber; (d) Steel, x7, La(NO3)3doped coating, organic acids treatment. PM observations pointed out both the optical quality and the resistance of coatings after the accelerated weathering tests were carried out. For instance, Figure 5shows the aspect of one of the glass slides coated with La(Ac) 3 doped silica after the most aggressive treatment under the Kesternich chamber conditions. Apart from the typical conchoidal fractures due to the glass piece cutting, no signs of alteration can be identified in the PM image, as well as in the corresponding OM image. Figure 5. Photograph, OM image and PM image of a glass slide piece coated with La(Ac) 3 doped silica after the treatment in the Kesternich chamber. All the coated samples were irradiated with UV light for at least 21 days, and after this treatment the coatings’ appearance upon metallic substrates is neutral, colorless and transparent, with the same aspect as before the irradiation, except for the steel substrates in which the coated area appeared slightly yellowish. Nevertheless, no deterioration signs were observed in any kind of samples. Concerning the optical quality of the coated samples, Vis transmission spectra recorded on glass slides coated with lanthanum-doped silica (Figure 6) show transmission percentages slightly higher than on the uncoated glass slide. This is attributed to the higher refractive index of the uncoated glass
Coatings 2018,8, 138 9 of 15 slide related to the lanthanum-doped silica coatings. Therefore, the optical quality of lanthanum-doped coatings is optimal to preserve the original appearance of metallic substrates in terms of brightness and reflection. Figure 6. Visible spectra of some of the samples studied. Black line: uncoated common glass slide. Blue line: glass slide coated with La(Ac) 3 doped silica. Red line: glass slide coated with La(NO 3 ) 3 doped silica. 3.4. Microstructural Features A selection of micrographs corresponding to the results after the most aggressive treatments are shown in this section for each kind of metallic substrate, even though all possible combinations of accelerated weathering tests and metallic substrates coated with the two lanthanum active dopants were carried out and observed by FESEM. In copper substrates after the treatment in the Kesternich chamber (Figure 7a), the uncoated area shows a heterogeneous surface of corrosion crust with quickly crystallized precipitates (Figure 7b), while in the coated area the sol-gel layer doped with La(NO 3 ) 3 appears cracked and a precipitate emerging from the metallic substrate is slowly formed near the cracks (Figure 7c). Figure 7. ( a ) FESEM image of a copper substrate in the coated/uncoated interface (La(NO 3 ) 3 doped coating) after the weathering test in the Kesternich Chamber; ( b ) Detail of the uncoated area; ( c ) Detail of the coated area.