scieee AI-readable full text Open interactive document viewer

New processing and applications of collagen containing calcium phosphate cements

Pérez Antoñanzas, Román

Abstract

When bone regeneration is needed, natural bone grafts are widely used. They are the best option since they present the same composition to that of bone, contain living cells with osteogenic potential, growth factors that induce cell differentiation into osteoblasts and extracellular matrix proteins that facilitate bone healing. However, this system presents some drawbacks, such as pain, morbidity, possible transmission of diseases in some cases, as well as limited availability. That is why synthetic bone grafts are one of the main objectives of the research in regenerative medicine and tissue engineering. This new discipline is based on the development of new biomaterials and on the comprehension of the interactions between the cells and the material in order to enhance the bone healing response. The present thesis is focused on calcium phosphate cements-based materials. CPC have the ability to transform an injectable paste made of calcium phosphates, into a phase similar to that of bone, hydroxyapatite. The CPC are well known for their osteoconductive properties. Nevertheless, these may be improved from a biological point of view and can be further processed to obtain materials with new morphologies and different applications. Therefore, the incorporation of collagen in these CPC was though as a way to enhance their biological performance. Furthermore, new processing approaches were studied, as well as their applications in new fields. The thesis is divided in three main parts: i) injectable composite cements; ii) composite macroporous scaffolds for tissue engineering and iii) composite microcarriers. In the first part, the fabrication of injectable composite cements is described as well their physico-chemical and morphological features. It is observed that the setting reaction is delayed in the presence of collagen during the initial minutes of reaction. Already after 1 hour the kinetics are similar in the presence and absence of collagen, without affecting the final product of reaction. The presence of collagen increases the injectability of the cements, whereas the mechanical properties decrease as the collagen concentration increases. From a biological point of view, the addition of collagen results in an increase in the initial cell adhesion as well as an increase in the cell proliferation rates. In the second part, macroporous scaffolds made of collagen and CPC are fabricated. These scaffolds are prepared through the freeze-drying of a collagen-CPC slurry. Different amounts of CPC are incorporated in the scaffolds. When mesenchymal stem cells are cultured on these scaffolds, it is observed that as the CPC content increases in the scaffolds, the cell differentiation increases, whereas the proliferation decreases. Further improvement of the scaffolds can be achieved though the incorporation of a BMP-7 gene into the scaffolds, in order to stimulate their osteoinductivity. The results show that as the gene incorporated in the scaffolds increases, there is an increase in the BMP-7 production, although this increase is associated with an increase in cell proliferation. In the third and final part, spherical microcarriers containing either gelatin or collagen are produced through the setting reaction of the CPC in a water in oil emulsion. The emulsion and CPC compositions can be adjusted in order to control the final features of the microcarriers. The in vitro characterization of the microcarriers reveals that under static and dynamic culturing conditions, microcarrieres are able to support cell attachment, proliferation and differentiation.

Full text

ADVERTIMENT . La consulta d’aquesta tesi queda condicionada a l’acceptació de les següents condicions d'ús: La difusió d’aquesta tesi per mitjà del servei TDX (www.tesisenxarxa.net) ha estat autoritzada pels titulars dels drets de propietat intel·lectual únicament per a usos privats emmarcats en activitats d’investigació i docència. No s’autoritza la seva reproducció amb finalitats de lucre ni la seva difusió i posada a disposició des d’un lloc aliè al servei TDX. No s’autoritza la presentació del seu contingut en una finestra o marc aliè a TDX (framing). Aquesta reserva de drets afecta tant al resum de presentació de la tesi com als seus continguts. En la utilització o cita de parts de la tesi és obligat indicar el nom de la persona autora. ADVERTENCIA. La consulta de esta tesis queda condicionada a la aceptación de las siguientes condiciones de uso: La difusión de esta tesis por medio del servicio TDR (www.tesisenred.net) ha sido autorizada por los titulares de los derechos de propiedad intelectual únicamente para usos privados enmarcados en actividades de investigación y docencia. No se autoriza su reproducción con finalidades de lucro ni su difusión y puesta a disposición desde un sitio ajeno al servicio TDR. No se autoriza la presentación de su contenido en una ventana o marco ajeno a TDR (framing). Esta reserva de derechos afecta tanto al resumen de presentación de la tesis como a sus contenidos. En la utilización o cita de partes de la tesis es obligado indicar el nombre de la persona autora. WARNING. On having consulted this thesis you’re accepting the following use conditions: Spreading this thesis by the TDX (www.tesisenxarxa.net) service has been authorized by the titular of the intellectual property rights only for private uses placed in investigation and teaching activities. Reproduction with lucrative aims is not authorized neither its spreading and availability from a site foreign to the TDX service. Introducing its content in a window or frame foreign to the TDX service is not authorized (framing). This rights affect to the presentation summary of the thesis as well as to its contents. In the using or citation of parts of the thesis it’s obliged to indicate the name of the author NEW PROCESSING AND APPLICATIONS OF COLLAGEN CONTAINING CALCIUM PHOSPHATE CEMENTS Román Pérez Antoñanzas 2011 Departament de Ciència de Materials i Enginyeria Metal · lúrgica Universitat Politècnica de Catalunya  ACTA DE QUALIFICACIÓ DE LA TESI DOCTORAL Reunit el tribunal integrat pels sota signants per jutjar la tesi doctoral: Títol de la tesi: ............................................................................................................... Autor de la tesi: .............................................................................................................. Acorda atorgar la qualificació de: No apte Aprovat Notable Excel·lent Excel·lent Cum Laude Barcelona, …………… de/d’….................…………….. de ..........…. El President El Secretari ............................................. ............................................ (nom i cognoms) (nom i cognoms) El vocal El vocal El vocal ............................................. ............................................ ..................................... (nom i cognoms) (nom i cognoms) (nom i cognoms)  UNIVERSITAT POLITECNICA DE CATALUNYA     New Processing and Applications of Collagen Containing Calcium Phosphate Cements Román Pérez Antoñanzas PhD Thesis Thesis supervisor: Prof Dra Maria Pau Ginebra Molins Departament de Ciencia dels Materials I Enginegyeria Metl·lurgica Escola tecnica superior d’enginyeria industrial de Barcelona Barcelona, 2011  I Acknowledgments Parece que fue ayer cuando empecé a trabajar en la tesis en el campo de los biomateriales. Esos fueron los comienzos de una nueva etapa o ciclo, y el ciclo finaliza aquí, con la lectura de la tesis. Durante estos años, de manera directa o indirecta, ha sido mucha la gente que ha contribuido para que esta llegase a su fin. Es por ello que estas personas se merecen unas líneas. En primer lugar se encuentra mi directora de tesis, Prof Maria Pau Ginebra. Ella es la que me ha guiado durante estos años. Le agradezco su paciencia y al mismo tiempo su nivel de exigencia. Este nivel de exigencia es lo que realmente me ha hecho esforzarme cada día al máximo para conseguir decir y hacer las cosas de la manera más eficiente. Sin embargo, lo que más le agradezco y lo que más valoro es el trato que ha tenido hacia mí, el entusiasmo y la alegría que me ha transmitido, las conversaciones del día a día. Por ello, aunque nuestras carreras científicas se separen, siempre recordaré que es una buena persona. Gracias. Al mismo tiempo, este comentario lo hago extensivo al Prof. Javier Gil quien, a pesar de que no he tenido interacción desde un punto de vista científico, siempre ha tenido el buen clima de trabajo y el buen ambiente en el grupo de investigación como prioridad y, sin duda, el lo ha sabido transmitir. Es por ello que el grupo de BIBITE es un sitio donde me he sentido a gusto, y agradezco a todas las personas que han contribuido a que reine este ambiente y que siempre me han animado durante la tesis. Es más, llegó un momento en que muchas de las personas dejaron de ser compañeros de trabajo para convertirse en amigos. Éste es el recuerdo con el que me quedaré durante muchos años. I’m also very thankful to Prof Myron Spector, for accepting me in his lab and for his kindness. He always had time for me, even in his busiest moments. He always had a smile for me and all the group members. For all his wise advices and his will to always help. I have great memories of the nine months I stayed in his lab in Boston. I also want to thank the rest of the people at tissue engineering lab for treating me as another member of the group. También me gustaría agradecer el trato recibido por el Prof Josep Anton Planell, el cual en su momento también me recibió con entusiasmo en el grupo y que también me ha permitido desarrollar parte de mi investigación en el centro que dirige, el IBEC. II También le agradezco la simpatía y alegría que siempre me ha transmitido. I would also like to thank George Altankov for all the advices he has given me and the discussions we have had that have helped me advance during these years. Agradecer a Jordi Franch y a todo su equipo de la facultad de veterinaria de la UAB por las implantaciones de los materiales desarrollados en la tesis. No simplemente el haber trabajado juntos, sino también el buen humor que tienen, a pesar de que las implantaciones fueron duras. Estos resultados no están incluidos en la tesis, pero es una gran satisfacción ver que los materiales pueden llegar a ser prometedores. Por supuesto que ha habido personas con las que he tenido más interacción que con otras y con las que he tenido grandes momentos, tanto dentro como fuera del trabajo. Los compañeros de la línea de cementos, Edgar, Gemma, Yassine, David, Montse, Cristina, Sara y Maite, con los cuales he interactuado con gran frecuencia y siempre han tenido buenos consejos. En su momento también fueron Sergio y Tania, los cuales me enseñaron mucho sobre los cementos en mis inicios. También a los estudiantes de ingeniería/master que hicieron el proyecto final conmigo y con los cuales trabajé más directamente codo con codo, como Kiara, Ferran y Cécile. Mis compañeros de despacho durante este final de tesis, Jordi, María, Noelia y Marta G, los cuales siempre han tenido palabras de apoyo, risas y sobretodo, buenos momentos. Marta P, que a pesar de no estar directamente en el mismo despacho, cada día tenía una sonrisa y aportaba más felicidad, si cabe, al despacho. Marc y Luis, con los que siempre compartía unas risas y los cuales siempre me animaban en todo lo que hacía. Txell, por ayudar siempre en todo lo que podía, por hacer los pedidos incluso antes de pedírselos y por su buena disposición. Pablo y Aleix por tener siempre buena predisposición. La gente con la que compartía buenos momentos en las comidas, en las cuales siempre, se hablara del tema del que se hablara, siempre reíamos. Me gustaría también tener unas líneas para la gente del IBEC con quien compartí buenas conversaciones y momentos. Miguel, del cual me acordaré siempre por su sonrisa constante y por ser una gran persona. Al lado de Miguel siempre estaba Óscar, y sabía que siempre que los veía juntos, dirían alguna de las suyas para estar riendo un rato. Eli, con la que también compartí buenos momentos. Melba, por la alegría constante que transmitía a la gente que estaba alrededor. Finalmente gente con la que IX Thesis objectives The aim of the thesis is to develop new materials with enhanced properties for bone regeneration. The thesis is based on calcium phosphate cements combined with collagen. Calcium phosphate cements have been widely studied, although the incorporation of this extracellular matrix protein has not been extensively investigated. Three specific objectives were established: - To fabricate an injectable calcium phosphate cement/collagen composite. - To fabricate macroporous collagen/calcium phosphate cement scaffolds for tissue engineering and gene delivery applications. - To fabricate hybrid calcium phosphate/gelatin or collagen microcarriers. These three main objectives can be considered as three different approaches to design biomaterials for bone regeneration. Relevant milestones can be identified within each of these three issues: 1. Fabrication of an injectable calcium phosphate cement/collagen composite - To optimize the L/P ratio to obtain an injectable and mouldable paste with good handling and setting properties. - To determine effect of collagen in the physico-chemical properties and morphology of the CPC. - To determine the effect of collagen concentration and its initial morphology in the CPC properties. - To determine the in vitro response of osteoblasts on the composite CPC. 2. Fabrication of macroporous collagen/calcium phosphate cement scaffolds for tissue engineering - To determine the effect of CPC incorporation in the collagen sponge properties. - To study the behavior of mesenchymal stem cells on scaffolds with different fractions of CPC. - To determine the effect of incorporating a bone morphogenetic protein 7 gene in the scaffolds on the mesenchymal stem cells response. X 3. Fabrication of hybrid calcium phosphate cement/gelatin or collagen microcarriers through a water in oil emulsion. - To optimize the processing parameters to obtain a low viscosity CPC paste adequate for microcarrier fabrication. - To introduce collagen or gelatin in the low viscosity CPC to fabricate composite microcarriers. - To optimize the emulsion parameters in order to obtain inorganic or composite microcarriers with desired features. - To determine in vitro cell viability of osteoblastic cells cultured on inorganic and composite microcarrier under static conditions. - To determine the ability of the microcarriers to be injected when mixed with an adequate gel. - To optimize in vitro conditions in spinner flask dynamic cultures to ensure cell viability on the microcarriers. XI Publications Espanol M, Pérez RA, Montufar EB, Marichal C, Sacco A & Ginebra MP. Intrinsic porosity of calcium phosphate cements and its significance for drug delivery and tissue engineering applications. Acta Biomaterialia 5 2752-2762 (2009). Ginebra MP, Espanol M, Montufar EB, Pérez RA & Mestres G. New Processing Approaches In Calcium Phosphate Cements And Their Applications In Regenerative Medicine. Acta Biomaterialia 6 2863–2873 (2010) Pérez RA, Del Valle S, Altankov G & Ginebra MP. Porous Hydroxyapatite and Gelatin/Hydroxyapatite Microspheres Obtained by Calcium Phosphate Cement Emulsion. Journal of Biomedical Biomaterials Research B: Applied Biomaterials 97 156-166 (2011). Perez RA, Ginebra MP & Spector M. Cell Response to Collagen-Calcium Phosphate Cement Scaffolds Investigated for Nonviral Gene Delivery. Journal of Materials Science: Materials in Medicine 22 887-897 (2011). Pérez RA, Altankov G, Jorge-Herrero E & Ginebra MP. Micro- and nanostructured hydroxyapatite/collagen microcarriers for bone tissue engineering applications. Journal of Tissue Engineering and Regenerative Medicine (submitted). Conference Participation Pérez RA, Del Valle S, Altankov G & Ginebra MP. Calcium Phosphate Cement Microcarriers. 8th World Biomaterials Congress 28th May- 1st June 2008, Amsterdam, Holland (Poster Presentation). Pérez RA, Del Valle S, Altankov G & Ginebra M.P. Desarrollo de microtransportadores de cement de fosfato de calcio para la regeneración ósea. X Congreso Nacional de Materiales 18-20th June 2008, San Sebastián, Spain (Oral Presentation). XII Pérez RA, Del Valle S, Altankov G & Ginebra MP. Hydroxyapatite and Hydroxyapatite/Gelatine Microcarriers Obtained by Calcium Phosphate Cement Emulsion. 2nd China-Europe Symposium on Biomaterials in Regenerative Medicine 16-20th November 2009, Barcelona, Spain (Oral Presentation). Pérez RA, Del Valle S, Altankov G & Ginebra MP. Porous Hydroxyapatite Microspheres as Cell Microcarriers for Bone Augmentation. The International Association for Dental Research General Session & Exhibition 14th-17th July 2010, Barcelona, Spain (Oral presentation). Pérez RA, Ginebra MP & Spector M. Collagen-Calcium Phosphate Cement Scaffolds for Nonviral Gene Delivery. 23rd European Conference on Biomaterials (ESB 2010) 11-15th September 2010, Tampere, Finland (Oral Presentation). Pérez RA, Ginebra MP & Spector M. Collagen-Calcium Phosphate Cement Scaffolds for Nonviral Gene Delivery. Symposium ITREN 2011 15th January 2011, Cheonan, South Korea (Oral Presentation). Acknowledgments I Abstract V Resumen VII Objectives IX Publications and Conference Participation XI Chapter 1: Introduction 1 1.1. Mythology and Science 1 1.2. Bone 3 1.2.1. Composition 3 1.2.1.1. Bone cells 4 1.2.2. Function 6 1.2.3. Structure 7 1.2.4. Bone remodeling 9 1.3. Bone substitutes 11 1.3.1. Bone graft 11 1.3.1.1. Autograft 12 1.3.1.2. Allograft 12 1.3.1.3. Xenografts 13 1.3.1.4. Synthetic Bone grafts 13 1.3.2. Tissue engineering and regenerative medicine 14 1.4. Biomaterials for bone tissue engineering and regenerative medicine 15 1.4.1. Calcium phosphates 15 1.4.2. Calcium phosphate cements 19 1.4.3. Collagen 21 1.4.4. Calcium phosphate/collagen composites for bone regeneration 24 1.5. Cell interactions with biomaterials 30 1.5.1. Collagen-integrins interaction 31 1.5.2. Recognition sites in triple helical and denatured collagen 33 1.6. References 34 Chapter 2: Calcium Phosphate Cement-Collagen for Bone Regeneration 49 2.1. Introduction 49 2.2. Objectives 51 2.3. Materials and methods 51 2.3.1. Powder phase 51 2.3.1.1. Synthesis and preparation 51 2.3.1.2. Characterization of powder 54 2.3.2. Liquid phase 55 2.3.2.1. Preparation of collagen solutions 55 2.3.2.2. Collagen characterization 56 2.3.3. Characterization of the setting reaction 57 2.3.3.1. Setting and cohesion times 57 2.3.3.2. Differential Scanning Calorimetry 59 2.3.3.3. pH evolution 59 2.3.4. Calcium phosphate cement properties 60 2.3.4.1. Collagen liberation during setting 60 2.3.4.2. Collagen distribution 61 2.3.4.3. Scanning electron microscopy 61 2.3.4.4. Fourier Transformed Infrared Spectroscopy 62 2.3.4.5. X-Ray diffraction 62 2.3.4.6. Helium pycnometry 63 2.3.4.7. Mercury intrusion porosimetry 63 2.3.4.8. Injectability 64 2.3.4.9. Mechanical properties 64 2.3.4.10. Statistical analysis 65 2.4. Results 65 2.4.1. Powder phase 65 2.4.1.1. Thermal treatment 65 2.4.1.2. Particle size distribution 66 2.4.2. Liquid phase 67 2.4.3. Characterization of the setting reaction 68 2.4.3.1. Setting and cohesion times 69 2.4.3.2. Differential scanning calorimetry 69 2.4.3.3. pH evolution 71 2.4.4. Calcium phosphate cement properties 73 2.4.4.1. Collagen release during the setting reaction 73 2.4.4.2. Collagen distribution 73 2.4.4.3. Scanning electron microscopy 76 2.4.4.4. Fourier Transformed Infrared Spectroscopy 78 2.4.4.5. X-Ray diffraction 82 2.4.4.6. Helium pycnometry 86 2.4.4.7. Porosimetry 87 2.4.4.8. Injectability 91 2.4.4.9. Mechanical properties 93 2.5. Discussion 95 2.5.1. Collagen processing 95 2.5.2. Setting reaction 98 2.5.3. Collagen release and collagen distribution 102 2.5.4. Microstructure 103 2.5.5. Phase evolution and CPC-collagen interaction 104 2.5.6. Density and porosity 106 2.5.7. Injectability 108 2.5.8. Mechanical properties 109 2.6. Conclusions 110 2.7. References 111 Chapter 3: Cell Response to Injectable CPC/Collagen Composites 121 3.1. Introduction 121 3.2. Objectives 122 3.3. Materials and methods 122 3.3.1. Materials 122 3.3.2. Cells 123 3.3.3. Cell behaviour on CPC/collagen composites 123 3.3.3.1. Initial adhesion 123 3.3.3.2. Cell proliferation and cell differentiation 124 3.3.4. Characterization 124 3.3.4.1. Proliferation 124 3.3.4.2. Differentiation 125 3.3.4.3. Fluorescence Diacetate staining 125 3.3.4.4. Scanning Electron Microscopy 126 3.3.5. Statistical analysis 126 3.4. Results 126 3.4.1. Initial cell adhesion 126 3.4.2. Cell proliferation and cell differentiation 128 3.4.2.1. Proliferation 128 3.4.2.2. Differentiation 129 3.4.2.3. Overall cell morphology 130 3.5. Discussion 132 3.6. Conclusions 136 3.7. References 137 Chapter 4: Cell Response to Collagen-Calcium Phosphate Cement Scaffolds Investigated for Nonviral Gene Delivery 141 4.1. Introduction 141 4.2. Objectives 143 4.3. Materials and methods 144 4.3.1. Collagen preparation 144 4.3.2. Calcium phosphate cement powder 144 4.3.3. Preparation of the scaffolds 144 4.3.3.1. Scaffold characterization 145 4.3.4. Plasmid preparation 145 4.3.5. MSC culture 147 4.3.6. In vitro behavior of scaffolds containing different HA content 147 4.3.6.1. Proliferation 148 4.3.6.2. Differentiation 148 4.3.6.3. Cell morphology 149 4.3.7. Plasmid incorporation 149 4.3.8. Statistical analysis 150 4.4. Results 150 4.4.1. Microstructure of the scaffolds 150 4.4.2. Plasmid characterization 152 4.4.3. Cell response to collagen scaffolds with different HA contents 153 4.4.4. BMP-7 expression 158 4.5. Discussion 160 4.6. Conclusions 164 4.7. References 165 Chapter 5: Porous Hydroxyapatite and Gelatin/Hydroxyapatite Microcarriers Obtained by Calcium Phosphate Cement Emulsion 171 5.1. Introduction 171 5.2. Objectives 174 5.3. Materials and methods 174 5.3.1. Microcarriers preparation 174 5.3.2. Microcarriers characterization 176 5.3.3. Cell cultures 177 5.3.3.1. Overall cell morphology 178 5.3.3.2. Cell proliferation 178 5.3.3.3. Cell differentiation 179 5.3.3.4. Statistical analysis 179 5.4. Results 179 5.4.1. Inorganic Microcarriers 179 5.4.2. Gelatine-Hydroxyapatite Microcarriers 183 5.4.3. Cellular response 185 5.5. Discussion 189 5.6. Conclusions 194 5.7. References 195 Chapter 6: Hydroxyapatite/collagen Microcarriers for Bone Tissue Engineering Applications 201 6.1. Introduction 201 6.2. Objectives 203 6.3. Materials and methods 203 6.3.1. Microcarrier preparation 203 6.3.2. Microcarriers characterization 204 6.3.3. In vitro culture test 205 6.3.3.1. Morphology 205 6.3.3.2. Cell proliferation 206 6.3.3.3. Cell differentiation 206 6.3.4. Statistical analysis 206 6.4. Results 206 6.4.1. Microcarrier characterization 206 6.4.2. In vitro culture test 209 6.4.2.1. Overall morphology and proliferation 209 6.4.2.2. Cell differentiation 212 6.5. Discussion 213 6.6. Conclusions 215 6.7. References 216 Chapter 7: Dynamic In Vitro Characterization CPC Composite Microcarriers 221 7.1. Introduction 221 7.2. Objectives 223 7.3. Materials and methods 223 7.3.1. Materials 223 7.3.2. Culturing cells on MC in dynamic cultures 223 7.3.2.1. Cell proliferation 226 7.3.2.2. Cell morphology 226 7.3.2.3. Statistical analysis 226 7.3.3. MC-containing alginate gels 227 7.4. Results 228 7.4.1. Dynamic culture 228 7.4.1.1. Short-time dynamic and static culture 229 7.4.1.2. Long-term dynamic and static culture 233 7.4.2. MC-containing alginate gels 236 7.5. Discussion 240 7.6. Conclusions 247 7.7. References 248 Conclusion and Future Perspectives 253 Chapter 1 7 The metabolic functionalities of bone are described on Table 1.3. Function Importance Mineral storage Act as reserves of minerals for the body, most notably calcium and phosphorous Growth factor storage Mineralized bone matrix stores important growth factors, such as insulinlike growth factors, transforming growth factors, bone morphogenetic proteins and others Fat storage The yellow bone marrow acts as a storage reserve of fatty acids Acid-base balance Buffers the blood against excessive pH changes by absorbing or releasing alkaline salts Detoxification Bone tissues can also store heavy metals and other foreign elements, removing them from the blood and reducing their effects on other tissues. These can later be gradually released for excretion Table 1.3. Metabolic functions of bone12. 1.2.3. Structure Bone is structured in a hierarchized form, and it is this hierarchy, that gives the optimum functional properties. The different levels at which bone may be studied can be observed in Figure 1.3.13: 1- The macrostructure: cancellous and cortical bone 2- The microstructure (from 10 to 500 µm): Haversian systems, osteons, single trabeculae 3- The sub-microstructure (1-10 µm): lamellae 4- The nanostructure (from hundred nanometers to 1 µm): fibrillar collagen and embedded mineral 5- Sub-nanostructure (below few hundred nanometers): molecular structure of constituent elements, such as mineral, collagen and non-collagenous organic proteins. 8 Introduction Figure 1.3. Structure of bone from its macrostructure to its sub-nanostrucuture13. This organization of bone and the resulting structure leads to excellent properties in the z direction, but with rather anisotropic and heterogeneous properties. At macroporous level, bone is distinguished between cortical or compact bone and cancellous or trabecular bone14. The end of a long bone has a dense cortical shell with a porous cancellous interior. As a first approximation, visual differences can appear when comparing cancellous and cortical bone, although the true differences appear at the microstructure. Cortical bone is composed of well structured osteons, which are concentrical structures on the center of which, the Haversian channels may be found. The sub-microstructure of cortical bone is composed of regular, cylindrically shaped lamellae. Each of the lamellas are composed of collagen fibers, and these collagen fibers, are the matrix onto which the HA may precipitate. The HA precipitates in the gaps left by the collagen, which are the gaps that are found between collagen fibers, separated by a typical 67 nm distance. Some researchers consider cortical and cancellous bone as a single morphological material which can be characterized by a highly variable porosity or apparent density15-17. In Chapter 1 9 general, cancellous bone is much more active metabolically, being remodeled much more often than cortical and therefore, can be considered as younger, on average, than the cortical bone. Cortical bone comprises 80% of the skeleton in mass and has a higher resistance to bending and torsion, due to its high density and its compact structure. The major part is calcified and its main function is to provide mechanical strength and protection. It can also participate in metabolic responses, particularly when there is severe or prolonged mineral deficit. On the other hand, trabecular bone represents 20% of the skeletal mass and is less dense, more elastic, and has a higher turnover than cortical bone, having a higher metabolic function. Trabecular bone serves as mechanical support in the case of vertebrae and provides the initial supplies in acute deficiency states18. It is important to take into account that the differences in structure will lead to differences in the mechanical behavior of bone and the values for maximum strength and Young modulus are shown in Table 1.4. Young Modulus (GPa) Compressive strength (MPa) Cortical bone 7-30 100-230 Cancellous bone 0.05-0.5 2-12 Table 1.4. Young modulus and compressive strength for cortical and cancellous bone19. 1.2.4. Bone remodeling Bone is a living organ that undergoes remodeling throughout life. Bone remodeling arises from the action of osteoblasts and osteoclasts that repair bone defects such as microfractures. In a hemostatic equilibrium, resorption and bone formation should be balanced, continuously replacing old bone by new bone formation. Bone remodeling is the process by which there is a bone turnover and that allows for bone to maintain the shape, quality and size of the skeleton. The remodeling cycle is shown in Figure 1.4 and consists of three consecutive phases: resorption, reversal and formation. The first phase, resorption, starts when partially differentiated mononuclear preosteoclasts migrate to the bone surface, where they form multinucleated osteoclasts. After the completion of this osteoclastic resorption, there is a 10 Introduction reversal phase where mononuclear cells appear on the bone surface. These cells are the ones that prepare the surface for new osteoblasts to begin bone formation and provide signals for osteoblasts differentiation and migration. The formation phase follows, with osteoblasts laying down bone until the resorbed bone is completely replaced by new one. When this phase is completed, the surface is covered with flattened lining cells and a prolonged resting period begins, until a new remodeling cycle is initiated. It has to be mentioned that the stages of remodeling cycle have different lengths. Resorption takes place probably in about 2 weeks, followed by 4 or 5 weeks for the reversal phase and finally, formation can take place for about 4 months, until the new bone is completely created. Figure 1.4. Representation of bone remodeling by osteoclasts and osteoblasts. Osteocytes are represented as mature osteoblasts which form part of the ECM12. The principle underlying bone remodeling is still unclear, but a well accepted theory for bone remodeling is based on the fact that bone has electrical properties, which is named piezoelectricity. Piezoelectricity is the coupling between mechanical deformation and electrical polarization of a material. The origin of piezoelectricity lies in the presence of asymmetric charged groups in the material. As the material is deformed, the charges move Chapter 1 11 respect to each other so that change in dipole moment occurs. It is collagen that gives the piezoelectric properties of bone. What happens in bone is that, when there is a tension or compression force, small electrical impulses are produced: the zones in which there is compression (concave parts of bone), these are charged negatively and new bone tissue is deposited in these zones, whereas in the zones that suffer tension (convex parts), these are positively charged and tissue is resorbed in this zone. This is the explanation for the monograph published in 1892 by Julius Wolff on bone remodeling, which is nowadays known as Wolff’s law and establishes that bone is reshaped in response to the forces acting on it20. 1.3. Bone substitutes 1.3.1. Bone graft The high regenerative capacity of bone previously explained due to its bone remodeling and since it is a dynamic system, makes it an ideal tissue for the healing of fractures without the need of a major intervention. This can only be applied in small fractures. In the case of having larger fractures, as those observed after bone tumors resections and nonunion fractures, the bone cells have no guide through which they can direct bone reconstruction. That is why these require a surgical intervention. Bone graft is the second most common transplanted tissue, being blood the first one. More than 500.000 bone grafting procedures are done annually in the United States and 2,2 million worldwide in order to solve injuries related to orthopedics, neurosurgery and dentistry21. Spinal fusions, filling defects following removal of bone tumors and several congenital diseases may require bone grafting. The gold standard of bone grafting is harvesting autologous cortical and cancellous bone from the iliac crest. Although autologous bone and other forms of bone grafting have disadvantages, and as such, their use is not optimal. The main properties that can be found in a bone graft from natural bone are briefly described, as well as the possible bone substitutes that can be used from other natural bones. 12 Introduction Osteogenesis, osteoinduction and osteoconduction are the three essential elements of bone regeneration, along with the osteointegration. Osteoprogenitor cells living within the donor graft could proliferate and differentiate to osteoblasts. These cells represent the osteogenic potential of the graft22. Osteoinduction is the stimulation and activation of host mesenchymal stem cells from the surrounding tissue, which differentiate into bone-forming osteoblasts. Osteoconduction is associated with the facilitation and orientation of blood vessel and the creation of the new Haversian systems into the bone scaffold. And finally, osteointegration describes the surface bonding between the host bone and the grafting material23. 1.3.1.1. Autograft Autograft is considered the gold standard since it provides optimal osteoconductivity and osteoinductivity, as well as osteogenic properties. Iliac crest is the most frequently chosen donor site as it provides easy access to good quality and quantity cancellous bone. Harvesting autologous bone from the iliac crest has disadvantages, such as pain and aesthetic deformities, as well as longer surgical procedures24-27. There is also the fact that most of the cellular elements will not survive the transplantation, which will reduce the osteogenic properties of the graft28. Besides this, autograft may also be associated with complications such as hematoma formation, blood loss, nerve injury, hernia formation, infection, arterial injury, urethral injury, fracture, pelvis instability, cosmetic defects, tumor transplantation, and sometimes chronic pain at the donor site24,26,29-32. 1.3.1.2. Allograft Allografts are grafts coming from an external donor and are considered as the most frequently chosen bone substitute33. It accounts for one third of bone grafts performed in the United States34. The benefit of using an allograft is that it avoids the pain from the donor site, but still presents some limitations and some risks. Allograft may carry the risk of transferring viral diseases. The allograft can be processed to reduce the risk, but in that case, the biological, such as its osteogenic potential, and mechanical characteristics can be reduced35-41. Chapter 1 13 Allograft can be prepared in fresh, frozen or freeze-dried forms, cortical or cancellous. Fresh allografts are rarely used, since they increase the probabilities to elicit an immune response or transmit diseases42. The concern regarding viral disease transmission is practically eliminated through tissue processing and sterilization. Freezing and irradiation that eliminate the cellular phase of the allograft modify the processes of graft incorporation and affect its structural strength. Frozen and freeze-dried allograft is more osteoconductive but is considered to have weak osteoinductive capabilities compared to fresh allograft. The method of preparation of the allograft is done in a way to reduce the risk of immune response, but eliminates any viable cells, reducing its osteogenic properties. The risk is still lower than in the case of blood transfer, but still exists43. It has been estimated that the risk of being infected with HIV virus in screened allograft is, 1 in 1,6 million, compared to that of blood, which is 1 in 450,000, which is still low, but existing34,44,45. 1.3.1.3. Xenografts Xenografts are derived from other species, having the organic components completely removed. Upon removal of the organic components, no possible immunological reaction can appear. The inorganic part, which is the only one remaining, can act as an structural scaffold, as well as a source of calcium46. The inorganic phase is also responsible for the physical dimension of the augmentation during remodeling phases47. Surgeons have used xenografts due to the introduction of a calcium phosphate source, offering the mechanical and architectural components of bone that lacked in the synthetics. Obviously, it fails to satisfy the standards set by autogenous bone because it does not have the organic or the cellular components. 1.3.1.4. Synthetic Bone grafts As was previously seen, autrografts seem very promising as bone grafts since they can provide support, fill voids and enhance biologic repair of skeletal defects. Although these promising characteristics, autografts present serious counterparts, such as donor site morbidity and the fact of not having enough amount or not in the adequate shape. That is why, nowadays, many synthetic bone grafts are under current investigations. Synthetic 14 Introduction bone graft materials are used in order to overcome the natural grafts drawbacks. In this sense, the materials are designed so that they meet similar features to those of natural grafts, such as osteoconductivty (e.g. calcium phosphates), osteoinductivity (e.g. incorporating growth factors) or osteogenicity (e.g. incorporating cells)48,49. 1.3.2. Tissue engineering and regenerative medicine Tissue engineering is a multidisciplinary field that involves chemistry, biology, medicine and materials science among others. This multidisciplinary implies applying principles and methods used in engineering as well as in biological sciences in order to understand the relationship between structure and function in tissues and develop biological substitutes which may be able to reestablish, maintain or improve a tissue50. The main idea is to overcome the limitations involved in the natural grafts and the simple implantation of biomaterials7. In order to do so, the basic principles of tissue engineering are shown in Figure 1.5, in which it can be seen that the process starts by extracting cells of the patient through a biopsy. These cells are then expanded in vitro and cultured afterwards on a scaffold or construct. The scaffold is then placed in a bioreactor to simulate the physiological conditions for cells to proliferate and differentiate into the cell lineage desired. The scaffold loaded with cells, is finally implanted into the patient. Figure 1.5. Scheme of tissue engineering principles. 1. Extraction of stem cells from the patient through a biopsy. 2. Expansion of cells in vitro. 3. Seeding the cells with growth factors on a scaffold. 4. Cell proliferation and differentiation ex vivo in a bioreactor to simulate physiological environment. 5. Implantation of the cell loaded scaffold on the patient51. Chapter 1 15 The materials implanted in the past were intended to be bio-inert. Scientist have now evolved to the fabrication of bioactive materials that integrate with biological molecules or cells and regenerate tissues7,52. The term regenerative medicine has similar concepts of those of tissue engineering, but with the only difference that in this case, the grafts or scaffolds can incorporate some type of signaling (e.g. growth factors) which will then be implanted by minimally invasive surgery into the defect. Therefore, in this approach, the scaffolds are implanted directly into the organism without the need of in vitro cultures53. 1.4. Biomaterials for bone tissue engineering and regenerative medicine Up to now, science has only been able to replace tissue with physiological tolerance, biocompatibility and long term stability, with relative success. This demonstrates that we are still far from obtaining a really biomimetic material and shows the superiority and complexity of natural structure54. It is important to distinguish the difference between a biological material and a biomaterial. Biological materials are the materials fabricated by biological systems, such as bones, whereas the biomaterials are materials that are designed and fabricated by scientist that can produce a beneficial effect on living tissues. In the latter case, biomimetic materials are a branch of biomaterials which are considered as biomaterials that are not made by living organisms, but have similar composition, structure and properties. 1.4.1. Calcium phosphates The use of calcium phosphates as bone biomaterial is due to the similarity with the mineral phase of bone and teeth. CaPs have been used for more than 90 years with medical objectives. The first CaP used for bone healing was proposed by Albee and Morrison in 192055. Later on, in 1951, Ray implanted HA in rats and Guinea pigs56. It was not until 1970, in which they started to be synthesized, characterized and implanted. 16 Introduction Calcium orthophosphates are considered as bioactive materials. The meaning for bioactive is that, these are materials that will promote the formation of a biological apatite before interfacing directly with the tissue at the atomic level, resulting in the formation of a direct chemical bond with bone. At the same time, in some cases CaP will be able to dissolve and allow newly formed tissue to grow. Bioceramics made of dense HA may be considered as bioactive, whereas porous scaffolds made of biphasic CaP, may be used as bioresorbable materials. The general applications of these materials are the use in non-loading bearing implants, such as filling bone defects in oral or orthopedic surgery, middle ear surgery or even coatings for metallic prosthesis. These materials are opposite to those considered as the first generation of biomaterials or bioinert, which would provoke the formation of a fibrous capsule isolating the material from the body. There are two main types of CaP: the ones obtained by precipitation of an aqueous solution at room temperature and the ones obtained by thermal treatment. The specific type of CaP that formed depends on the solubility of the CaP in aqueous medium. The name and composition of the main compounds that can be obtained at low temperature in aqueous systems, as well as the compounds obtained by thermal treatment, appear in Table 1.5: Name Formula Ca/P Mineral Symbol Monocalcium phosphate monohydrate Ca(H 2 PO 4 ) 2 ·H 2 O 0.50 - MCPM Dicalcium phosphate CaHPO4 1.00 Monetite DCP Dicalcium phosphate dihydrate CaHPO 4 ·2H 2 O 1.00 Brushite DCPD Octacalcium phosphate Ca8H2(PO4)6·5H2O 1.33 - OCP Precipitated hydroxyapatite Ca 10-x (HPO 4 ) x (PO 4 ) 6-x (OH) 2-x 1.33- 1.67 - PHA Precipitated amorphous calcium phosphate Ca 3 (PO 4 ) 2 ·nH 2 O where n=3-4.5 1.50 - ACP Monocalcium phosphate Ca(H2PO4)2 0.50 - MCP α-Tricalcium phosphate α-Ca3(PO4)2 1.50 - α-TCP β-Tricalcium phosphate β-Ca3(PO4)2 1.50 - β-TCP Sintered hydroxyapatite Ca10(PO4)6(OH)2 1.67 Hydroxyapatite SHA Oxyapatite Ca10(PO4)6O 1.67 - OXA Tetracaclium phosphate Ca4(PO4)2O 2.00 Hilgenstockite TetCP Table 1.5. Calcium phosphates that may be obtained at low temperature (top 6) or through high temperature sintering (bottom six)57. Chapter 1 23 bundles, making collagen stronger and more stable. The main advantages and some drawbacks for using collagen are summarized in Table 1.7. Advantages Disadvantages Available in abundance and easily purified from living organism. High cost of pure type I collagen. Non-antigenic. Variability of isolated collagen. Biodegradable and bioresorbable. Hydrophyilicity which leads to swelling and more rapid release. Non-toxic and biocompatible. Variability in enzymatic degradation rate as compared with hydrolytic degradation. Synergic with bioactive components. Complex handling properties. High tensile strength. Side effects, such as bovine spongiform encephalopathy. Hemostatic: promotes blood coagulation. Different forms. Biodegradability can be regulated by cross-linking. Easily modifiable to produce materials as desired using its functional groups. Compatible with synthetic polymers. Table 1.7. Advantages and disadvantages of using collagen as biomaterial78. In the field of bone regeneration, collagen has been used, although due to its low mechanical properties it has been usually combined with other materials such as HA, which in addition can make the material osteoinductive under certain enviorments79,80. Nevertheless, it is not the only way collagen can be made osteoinductive, since it has also been used in some occasions as drug carrier (e.g. BMP-2) in order to induce bone cell differentiation81. In order to reproduce the function needed, it is important to recreate the bone ECM structure. The structure of the ECM is basically composed of collagen, and that is why, many efforts have been put on developing systems which are able to recreate the appropriate bone ECM micro-architecture. That is why, collagen gels are used to create tissue equivalents. The properties of this gel will depend on the organization of the collagen fibrils in the network, which at the same time is a response of external stimuli, such as mechanical stimuli. These fibril gels create a 3D network on which cells can be seeded, which may promote in vivo like cellular activity that is completely different from those observed in 2D82. 24 Introduction 1.4.4. Calcium phosphate/collagen composites for bone regeneration There are many studies in which collagen has been mixed with hydroxyapatite. These composites may present advantages over the different components individually. An accelerated osteogenesis was observed in a study in which collagen/HA scaffolds were implanted in Wistar rats in 5 mm calvariae defects and were shown to increase osteogenesis already after 28 days80. Other collagen/HA composite material has also shown better osteoconductive properties and calcification production identical to that of bone matrix83,84, presenting biocompatibility both, in animals and humans, as was observed in commercially available composites (Biostite and Bio-Oss)83,85. Mehlisch in the 90s, implanted a material composed of a collagen matrix with HA particles for ridge augmentation for 1 year and reported a high biocompatibility86. Besides the enhanced biological behavior, the composite mechanically may also behave in a better way than its components by themselves. The ductile properties of collagen may help increasing the low fracture toughness of ceramics. On the other hand, the addition of a ceramic in collagen has also been reported to have an increased resistance to three dimensional swelling compared to collagen as observed in a collagen calcium phosphate composite in the form of multilayer sheets obtained using enzymatic mineralization87. They have been also shown to improve its mechanical wet properties88. Compared to other scaffolds, there is evidence of the biological advantage of collagen compared to artificial polymeric scaffolds, demonstrated in cartilage regeneration89, as well as a better cell adhesion to collagen surfaces rather than PLLA or PGA implants90. Some polymeric scaffolds can take up to two years to degrade (e.g. Poly(hydroxybutyrate) (PHB), Poly(hydroxyvalerate) (PHV))91, while some collagen hydroxyapatite composites have a more reasonable degradation rate between 2 months and 1 year92. On the other hand, when comparing hydroxyapatite/collagen composite scaffolds to other ceramic scaffolds, they perform well compared to HA or TCP89. The addition of collagen to the ceramic structure can provide improvements from a surgical point of view: shape control, spatial adaptation, Chapter 1 25 increased particle and defect wall adhesion and the capability to favor clot formation and stabilization 85. A synthetic bone graft substitute of type I bovine collagen, hydroxyapatite and tricalcium phosphate (Collagraft Bone graft matrix Strip) was used successfully in animal and human applications for long bone fractures93. It was approved by FDA in 1994 as a substitute for autogenous bone grafts for treating acute long bone fractures and traumatic defects when used with bone marrow and internal or external fixation. It was reported as a highly compatible and well incorporated in spinal fusion93. However, Muschler et al94 reported the use of Collagraft in a canine spinal fusion model stabilized with acrylic bone cement and cerclage wire. They reported poor results, mainly attributed to poor stabilization of the spine through cement and cerclage wire fixation. Nowadays, some biomaterials composed of hydroxyapatite and collagen may be found in the literature. The processes by which these are obtained differ among them and this leads to different final properties. The intention of the following paragraphs is to give an overview of the different techniques that are being used and that have been used for the preparation of hydroxyapatite and collagen composites. a) Soaking of collagen sponges The method consists on the immersion of a collagen porous matrix in a phosphate containing solution, mainly SBF or PBS, in order for the HA to precipitate. The HA crystals are able to precipitate on and throughout the collagen matrix. The collagen is usually lyophilized in order to obtain a porous sponge like morphology. The majority of these scaffolds are based on the method described by Kokubo95. When the fluid in which the collagen sponge is located becomes supersatured in calcium and phosphates ions, such as when placed in SBF solution, HA precipitates on top of it96,97. It is considered as a fast and easy method to obtain a collagen HA scaffold. In this approach, the first experiments were done with SBF or PBS as mentioned, but since then, new solutions have arisen in order to also obtain HA which may affect the final properties of the HA98. In general, it is difficult to control the amount of HA that is incorporated into the scaffolds. 26 Introduction An upgrade of this principle consists on placing the collagen sponge in water and make calcium and phosphate solutions pass through the sponge drop by drop. Collagen has a solid form, making a calcium phosphate solution diffuse into the fibrils88. It is reported that in this way, the orientation of the collagen fibers can be controlled99. Furthermore, by controlling the solutions used and the speed at which the solutions are added, a gradient collagen scaffold with calcium rich areas and calcium depleted areas can be obtained100. An even more interesting approach that was taken in a previous work was to create sponges with the soaking method and then incorporating cells arising from bone fragments. This sponges were then able to be coiled, obtaining scaffolds colonized with cells even in the inside of the scaffold101. The use of a sponge is not always necessary. In another example, microbeads of collagen were prepared, and in order to stabilize the structure, these were crosslinked with glutaraldehyde and placed in PBS for the precipitation of the HA102. Nevertheless, even though the majority of scaffolds are obtained having a collagen scaffold onto which the HA is precipitated, the opposite can also be found, in which a porous HA scaffold can be made, being impregnated afterwards with a collagen solution103. b) Simultaneous precipitation of calcium phosphate/collagen solutions Many other works relay on the principle of a simultaneous precipitation of collagen and HA. The condition for the stable formation of HA is alkaline, and collagen fibrillogeneis occurs at around body temperature and pH. That is why, for the fibrillogeneis of collagen to occur in vitro, it requires certain conditions of physiological saline with a precise pH and temperature104,105. In order to obtain this simultaneous precipitation, the process is generally done through a simultaneous titration system. There are several ways through which this co-precipitation can be obtained. The system can be formed by a phosphate containing solution and collagen solution106, or a calcium containing and collagen solution104. This way, both the Chapter 1 27 collagen and the HA will precipitate at the same time. That is why the system is called coprecipitation or simultaneous precipitation. It has been demonstrated that the c-axis of HA crystals can be induced to grow along the direction of collagen fibrils, if the right conditions of mineralization are met, in which the temperature is maintained at 40ºC and the pH around 8-9107. The system by which it is prepared is similar to that shown in Figure 1.10. The way in which the experiment was carried out, was having 2 l of 99.6 mM Ca(OH)2 aqueous suspension and another tank with 2 l of 59.7 mM H3PO4 aqueous solution with 5 grams of atelocollagen. Both solutions were added drop by drop in a central tank, which initially contained 1 l of water. These concentrations were established in order to obtain a final weight ratio of HA/col of 80/20. The temperature was controlled in a water bath, and so was the pH by the simultaneous titration of Ca2+ and PO43- solutions106,107. The solutions concentration is usually controlled so that the final ratio of HA/col is between 80/20 and 60/40 (wt/wt)107-110. Figure 1.10. Representation of the system used to prepare scaffolds through a co-precipitation of collagen with calcium and phosphate ions107. The results showed the fabrication of collagen fibers of 20 µm in length and having the caxes of HA crystals aligned along the elongation direction of the HA/col fibers, which is similar to the structure found in bone111. The driving force for the surface interaction between HA and collagen was probably an interfacial interaction between these molecules, because HA formation on Langmuir-Blodgett monolayers indicates that HA nanocrystals 28 Introduction formed on carboxyl-terminated monolayer, but not formed on amino-terminated monolayer112. Red shifts were observed with FTIR when comparing the collagen spectra with those of the composites. Those shifts are related with a decrease in bonding energy of the C-O bond and is basically assumed to be caused by the interaction with Ca2+ ions. This method has been resembled by other authors by using similar protocols in which the collagen and the HA precipitate at the same time113. c) Solid freeform fabrication The use of solid freeform fabrication for collagen/HA scaffolds has not been directly applied to collagen slurries, but rather, moulds made of polymeric materials have been prepared with the solid freeform fabrication technique, onto which the collagen/HA slurries were then poured. Briefly, collagen slurries containing 70% wt of HA were mixed and blended. These slurries were then poured into the moulds fabricated through solid freeform fabrication of biocompatible materials (BioBuild and BioSupport). The moulds with the slurries were then frozen and after the complete freezing, these were immersed in ethanol for the complete dissolution of the moulds. The materials were then left drying in order to obtain the macroporous scaffolds. It is important to highlight that the morphology and porosity of the scaffolds completely depends on the solid freeform fabricated mould114-116. d) Freeze-dried collagen and HA slurries This method is also called the phase separation method or simply freeze-drying process. It is based on the freeze-drying of collagen:HA slurries to obtain macroporous scaffolds. The techniques described up to now usually had the collagen as the matrix of the material. With the present technique, materials with higher content of HA can be obtained. This means that in the case in which the amount of collagen is high, and therefore, becomes the continuous phase, the material obtained will be a highly porous material with HA deposits. In the case in which the amount of HA is high, the material obtained will be a ceramic with some collagen, not presenting, in general, macroporosity. The ratios of HA and collagen can be perfectly controlled by controlling the amount of HA incorporated81,117-120. In the previously described methods, since HA arises from precipitation, the amount of HA is more difficult to control and is generally between 80:20 or 60:40 wt ratios of HA:collagen. Chapter 1 29 With the present technique, most of the works present a higher range of HA:collagen weight ratios, ranging from 1:99 to 2:181,119. Higher ranges have also been covered up to a 8:1 weight ratio of HA:collagen content in collagen scaffolds120. TenHuisen also obtained a composite with a higher ratio of HA in the composite, being HA the matrix of the material, achieving up to a 22:1 HA:collagen weight ratio121. e) Calcium phosphate cements with collagen There have been few works in which collagen has been combined with a CPC. An apatitic CPC composed of TTCP/DCP was studied in combination with collagen at a L/P ratio of 0.29 ml/g, adding collagen in its liquid and its powder phase122. The results showed that the incorporation of the collagen in the powder phase gave poor results in terms of setting time. Lower setting times were found when collagen was incorporated in the liquid phase, although the optimum results were found when the liquid phase was composed of collagen and an accelerant solution (e.g. sodium hydrogenphosphate). There was an increase in the setting time and a linear decrease in the diametral tensile strength when collagen was present in more than 1% in the liquid phase. When the accelerant solution was present, there was an improvement in workability and handling122. More recent works describe the addition of collagen (3% wt) in the liquid phase in a brushitic cement composed of MCP and β-TCP123 at a L/P ratio of 0.29 ml/g and also reported an improvement in cement handling. Furthermore, collagen was found to accelerate the setting reaction and maintain the compressive strength similar to that of the cement without collagen. The most important claim was the excellent cohesion properties and high cellular adhesion123. An even more recent work reports a 10 fold increase in the work of fracture of an apatitic CPC composed of TTCP and DPA containing 5% collagen solution in its liquid phase for different L/P (e.g. 0.29, 0.33 and 0.4 ml/g)124. Furthermore, the presence of collagen doubled the initial cellular attachment in the composite at a L/P ratio of 0.29 ml/g for collagen concentrations of 2.5 and 5% wt124. Recent work also describes the hydrolysis of a collagen and α-TCP paste in water125. Two different methods for the mixing were applied: simple mixing or milling the mixture, using 5% and 20% weight collagen ratios respect to HA. It was shown that in the case of having the non-milled composite, the diametral tensile strength decreased compared to HA alone, whereas it remained similar in the case of the milled case. The 30 Introduction diametral tensile strength was higher in the case of the milled composite compared to the non-milled composite and is attributed to the better dispersion of small collagen fibers in the composite125. 1.5. Cell interactions with biomaterials The adhesion of cells to biomaterials is affected by the characteristics of the materials surface, which includes the chemistry, topography, surface energy, etc. All these parameters play an important role in the subsequent capacity of the cells to proliferate and differentiate, as well as to attach, adhere and spread on the initial stages. The behavior of the cells in the first stages of culture, will rule the posterior behavior of cells on the biomaterial. There are several mechanisms by which cells are able to communicate among them126 and with the surface of the ECM127 (or to the surface of a material in which proteins have been deposited), which will determine the way in which the cells will behave. There is a high specificity between the ligands and the adhesive molecules. The ligands may be in the surface of the material or in neighboring cells. There are four families of adhesion molecules: selectins, immunoglobulin superfamily, cadherins and integrins. Only cadherins and integrins have been described in osteoblastic cells. Integrins are the adhesion molecules that deal with cell substrate adhesion, while cadherins control cell to cell adhesions. We will only briefly describe the integrins since these are the only ones that will actually be discussed during the thesis. Integrins consist of transmembrane heterodimers formed by the union of α and β subunits. Each of the subunits presents a large extracellular domain, transmembrane domain and a short cytoplasmatic domain. These heterodimers are the ones that will send the information found outside the cells, inside, meaning that it will control the adhesion, spreading, proliferation, differentiation and even the apoptosis of the cell128- 130. The linking between the integrin receptors and the substratum of the material are the so called focal contacts. These focal contacts are closed junctions where the distance between the substrate surface and the cell membrane is between 10 – 15 nm. A focal contact occurs Chapter 1 31 essentially in cells with low motility and is promoted in vitro by ECM proteins, like fibronectin and vitronectin. These focal contacts and the subsequent architecture of the cytoskeleton will determine the mobility and the strength of the adhesion. In this context, if the architecture of the cytoskeleton is in the shape of long bundles, presenting finger like protrusions, they are called fillopodia. If they are assembled in the form of a mesh and the structure of the protrusions is sheet like, they are called lamellipodia. It can be said that cells with a low motility present strong focal adhesions, whereas the ones with a high motility, form less adhesive structures. It will be the surface characteristics of the material, as well as the capacity to attract proteins to its surface, that will determine the cell morphology. Cells will initially attach, adhere and finally spread. In the case of having a calcium phosphate cement, the ability to adsorb proteins on its surface will arise from the surface energy of the CDHA formed and from the high specific surface area, among other parameters, to attach proteins. Cells will be able to interact with the adsorbed proteins. The hypothesis is that by adding collagen on the structure of the CPC, there will be an increase of the chance for the cells to find a binding domain on the surface, through which cells will adhere. 1.5.1. Collagen-integrins interaction Integrins is a term which was first applied in 1987 to emphasize the role of these receptors in integrating the extracellular matrix outside the cell with the actin containing cytoskeleton inside the cell. The signals they convert travel two directions: from outside the cell, inside, and the other way round as well. They transduce information from the ECM to the cell and reveal the status of the cell to the ECM. This allows cells to make rapid and flexible responses. Integrins are the largest family of cell adhesion receptors131. Integrin type receptors are composed of one α and one β subunit. They are transmembrane proteins and are not covalently linked together. Integrin α, has 5 subunits, only presenting 4 of them in vertebrates132. The largest subgroup on vertebrates is formed by α subunits that have a special ligand binding inserted domain, named αI domain. There are four integrins 32 Introduction containing αI domain (subunits α1, α2, α10 and α11) for the collagen receptor integrins. These types of units have associated a β1 heterodimer. The most important and well known are α1β1 and α2β1. Integrin α1β1 is expressed in many MSC and seems to be important for the action of many inflammatory cells. Integrin α2β1 is abundant on many epithelial cells types and platelets and is also expressed in MSC. These two integrins may have opposite effects on many signaling pathways133-135. It is also well known that, depending on the type of collagen, the integrins also have different affinities (Figure 1.11). In other words, the type of integrin interaction may depend on the type of collagen. In this sense, α2 and α11, have a higher affinity for the fibril forming collagens, such as types I, II and III, whereas, α1 and α10 have higher affinity for basement membrane (type IV) and beaded filament (VI) collagens. At the same time, the response that is given from the outside to the inside of the cell will also depend on the type of integrin that is being activated. In the case of α1, the proliferation is increased, whereas the collagen synthesis is decreased, whereas for α2, collagen synthesis is increased and so is the collagenase synthesis increased. In the case of α10 and α11 the effects are unknown. Figure 1.11. Representation of integrins involved in the collagen interaction with cells132. Chapter 1 39 53. Spine JD. Tissue engineering and reparative medicine. Annals New York Academy of Sciences 961, 1-9 (2002). 54. Vallet-Regi M & Gonzalez-Calbet JM. Calcium phosphates as substitution of bone tissues. Progress in Solid State Chemistry 32, 1-31 (2004). 55. Albee FH & Morrison HF. Studies in bone growth - Triple calcium phosphates as a stimulus osteogenesis. Annals of Surgery 71, 32-39 (1920). 56. Ray RD, Degge J, Gloyd P & Mooney G. Bone regeneration - an experimental study of bone grafting materials. Journal of Bone and Joint Surgery - American Volume 34A, 638-647 (1952). 57. Driessens FCM & Verbeeck RMH. Biominerals. CRC Press, Florida (1990). 58. Driessens F & Verbeeck R. Implant materials in biofunction. Advances in biomaterials. de Putter C, de Lange GL, de Groot K & Lee AJC (eds.), pp. 105-111 Elsevier, Amsterdam,1998. 59. Van Wazer JR & Gilchrist R . Phosphorous and its compounds. Science 129, 1271- 1272 (1985). 60. Chow LC. Development of self-setting calcium phosphate cements. Journal of the Ceramic Society of Japan. International Edition 99, 927-936 (1992). 61. Driessens FC, Planell JA, Boltong MG, Khairoun I & Ginebra MP. Osteotransductive bone cements. Proceedings of the Institution of Mechanical Engineers, part H: Journal of Engineering in Medicine 212, 427-435 (1998). 62. Frankenburg EP et al. Biomechanical and histological evaluation of a calcium phosphate cement. The Journal of Bone and Joint Surgery 80, 1112-1124 (1998). 63. Frayssinet P, Gineste L, Conte P, Fages J & Rouquet N. Short-term implantation effects of a DCPD-based calcium phosphate cement. Biomaterials 19, 971-977 (1998). 40 Introduction 64. Ginebra MP. Orthopaedic bone cements. Deb S (ed.), pp. 206-230 CRC Press Woodhead Publishing limited, Cambridge, 2008. 65. Dorozhkin SV. Calcium orthophosphate cements for biomedical application. Journal of Materials Science 43, 3028-3057 (2008). 66. LeGeros RZ, Chohayeb A & Shulman A. Apatitic calcium phosphates: possible dental restorative materials. Journal of Dental Research 61, 343-347 (1982). 67. Brown WE & Chow LC. A new calcium phosphate setting cement. Journal of Dental Research 62, 672-679 (1983). 68. Brown W & Chow L. Dental restorative cement pastes. Patent-4518430 (1985). 69. Driessens FC, Boltong MG & Bermudez O. Formulation and setting times of some calcium orthophosphate cements: a pilot study. Journal of Materials Science: Materials in Medicine 4, 503-508 (1993). 70. Chow LC, Markovic M & Takagi S. Cements research progress. LJ Struble (ed.), pp. 215-238 American Ceramic Society, Watersville, OH,1998. 71. Driessens FCM et al. Effective formulations for the precipitation of calcium phosphate bone cements. Journal of Materials Science: Materials in Medicine 5, 164-170 (1994). 72. Ramachandran GN & Reddi AH. Biochemistry of collagen. Plenum, New York (1976). 73. Traub W & Piez KA. Advances in protein chemistry. CB Anfinsen, JT Edsalla & FM Richards (eds.), pp. 245 Academic Press, New York,1971. 74. Nimni ME & Harkness RD. Collagen Biochemistry, vol I. ME Nimni (ed.), pp. 1-79 CRC Press, Boca Raton,1988. Chapter 1 41 75. Kramer RZ, Bella J, Mayville P, Brodsky B & Berman HM. Sequence dependent conformational variations of collagen triple-helical structure. Nature Structural Biology 6, 454-457 (1999). 76. Mayne R & Burgenson RE. Structure and function of collagen types. Academic, Orlando, Florida (1987). 77. McPherson JM, Sawamura S & Amstrong R. An examination of the biological response to injectable, glutaraldehyde cross-linked collagen implants. Journal of Biomedical Materials Research 20, 93-107 (1986). 78. Lee CH, Singla A & Lee Y. Biomedical applications of collagen. International Journal of Pharmaceutics 221, 1-22 (2001). 79. Takaoka K, Nakahara H & Yoshikawa H. Ectopic bone induction on and in porous hydroxyapatite combined with collagen and bone morphogenetic protein. Clinical Orthopaedics 234, 250-254 (1988). 80. Gleeson JP, Plunkett NA & O'Brien FJ. Addition of hydroxyapatite improves stiffness, interconnectivity and osteogenic potential of a highly porous collagenbased scaffold for bone tissue regeneration. European Cells and Materials 20, 218- 230 (2010). 81. Murata M et al. Bone augmentation by recombinant human BMP-2 and collagen on adult rat parietal bone. International Journal of Oral Maxillofacial Surgery 28, 232- 237 (1999). 82. Pedersen JA & Swartz MA. Mechanobiology in the third dimension. Annals of Biomedical Engineering 33, 1469-1490 (2005). 83. Serre CM, Papillard M, Chavassieux P & Boivin G. In vitro induction of a calcifying matrix by biomaterials constituted of collagen and/or hydroxyapatite: an ultrastructural comparison of three types of biomaterials. Biomaterials 14, 97-106 (1993). 42 Introduction 84. Wang RZ et al. Synthesis of nanophase hydroxyapatite collagen composite. Journal of Materials Science Letters 14, 490-492 (1995). 85. Scabbia A & Trombelli L. A comparative study on the use of a HA/collagen/chondroitin sulphate biomaterial (Biostite®) and a bovine-derived HA xenograft (Bio-Oss®) in the treatment of deep intraosseous defects. Journal of Clinical Periodontology 31, 348-355 (2004). 86. Mehlisch DR, Leider AS & Roberts WE. Histologic evaluation of the bone/graft interface after mandibular augmentation with hydroxylapatite/purified fibrillar collagen composite implants. Oral Surgery, Oral Medicine, Oral Pathology, Oral Radiology, and Endodontology 70, 685-692 (1990). 87. Yamauchi K, Goda T, Takeuchi N, Einaga H & Tanabe T. Preparation of collagen/calcium phosphate multilayer sheet using enzymatic mineralization. Biomaterials 25, 5481-5489 (2004). 88. Lawson AC & Czernuszka JT. Collagen-calcium phosphate composites. Proceedings of the Institution of Mechanical Engineers, part H: Journal of Engineering in Medicine 212, 413-425 (1998). 89. Wang X et al. Tissue engineering of biphasic cartilage constructs using various biodegradable scaffolds: an in vitro study. Biomaterials 25, 3681-3688 (2004). 90. El-Amin SF et al. Extracellular matrix production by human osteoblasts cultured on biodegradable polymers applicable for tissue engineering. Biomaterials 24, 1213- 1221 (2003). 91. Kohn J, Abramson S & Langer R. Biomaterials Science. Ratner BD, Hoffman AS, Schoen FJ & Lemons JE (eds.), pp. 115-127 Elsevier, San Diego,2004. 92. Johnson KD et al. Porous ceramics as bone graft substitutes in long bone defects: a biomechanical, histological, and radiographic analysis. Journal of Orthopaedic Research 14, 351-369 (1996). Chapter 1 43 93. Walsh WR et al. Mechanical and histologic evaluation of Collagraft in an ovine lumbar fusion model. Clinical Orthopaedics and Related Research 375, 258-266 (2000). 94. Muschler GF et al. Evaluation of collagen ceramic composite graft materials in a spinal fusion model. Clinical orthopaedics and Related Research 328, 250-260 (1996). 95. Kokubo T, Kushitani H, Sakka S, Kitsugi T & Yamamuro T. Solutions able to reproduce in vivo surface-structure changes in bioactive glass-ceramic A-W. Journal of Biomedical Materials Research 24, 721-734 (1990). 96. Lickorish D, Ramshaw JAM, Werkmeister JA, Glattauer V & Howlett CR. Collagen-hydroxyapatite composite prepared by biomimetic process. Journal of Biomedical Materials Research 68A, 19-27 (2004). 97. Zhang LJ et al. Hydroxyapatite/collagen composite materials formation in simulated body fluid environment. Materials Letters 58, 719-722 (2004). 98. Goes JC et al. Apatite coating on anionic and native collagen films by an alternate soaking process. Acta Biomaterialia 3, 773-778 (2007). 99. Iijima M, Moriwaki Y & Kuboki Y. Oriented growth of octacalcium phosphate on and inside the collagenous matrix in vitro. Connective Tissue Research 32, 519-524 (1996). 100. Chaozong L, Zhiwu H & Czernuszka JT. Gradient collagen/nanohydroxyapatite composite scaffold: Development and characterization. Acta Biomaterialia 5, 661- 669 (2009). 101. Du C, Cui FZ, Zhu XD & de Groot K. Three-dimensional nano-HAp/collagen matrix loading with osteogenic cells in organ culture. Journal of Biomedical Materials Research 44, 407-415 (1999). 44 Introduction 102. Tsai SW, Hsu FY & Chen PL. Beads of collagen-hanohydroxyapatite composites prepared by a biomimetic process and the effects of their surface texture on cellular behavior in MG63 osteoblast-like cells. Acta Biomaterialia 4, 1332-1341 (2008). 103. Teixeira S, Fernandes MH, Ferraz MP & Monteiro FJ. Proliferation and mineralization of bone marrow cells cultured on macroporous hydroxyapatite scaffolds functionalized with collagen type I for bone tissue regeneration. Journal of Biomedical Materials Research 95A, 1-8 (2009). 104. Jens-Hilmar B, Michael M, Angelika T & Wolfang P. Biomimetic mineralization of collagen by combined fibril assembly and calcium phosphate formation. Chemistry of Materials 11, 2694-2701 (1999). 105. Zhang W, Liao SS & Cui FZ. Hierarchical self-assembly of nano-fibrils in mineralized collagen. Chemical Materials 15, 3221-3226 (2003). 106. Kikuchi M et al. Biomimetic synthesis of bone-like nanocomposites using the selforganization mechanism of hydroxyapatite and collagen. Composites Science and Technology 64, 819-825 (2004). 107. Kikuchi M, Itoh S, Ichinose S, Shinomiya K & Tanaka J. Self-organization mechanism in a bone-like hydroxyapatite/collagen nanocomposite synthesized in vitro and its biological reaction in vivo. Biomaterials 22, 1705-1711 (2001). 108. Yoshida T, Kikuchi M, Koyama Y & Takakuda K. Osteogenic activity of MG-63 cells on bone-like hydroxyapatite/collagen nanocomposite sponges. Journal of Materials Science: Materials in Medicine 21, 1263-1272 (2010). 109. Toh S et al. Development of an artificial vertebral body using a novel biomaterial, hydroxyapatite/collagen composite. Biomaterials 23, 3919-3926 (2002). 110. Song JH, Kim HE & Kim HW. Collagen-Apatite nanocomposite membranes for guided bone regeneration. Journal of Biomedical Materials Research: Applied Biomaterials 83B, 248-257 (2007). Chapter 1 45 111. Sasaki N & Sudoh Y. X-ray pole figure analysis of apatite crystals and collagen molecules in bone. Calcified Tissue International 60, 361-367 (1997). 112. Sato K, Kumagai Y & Tanaka J. Apatite formation on organic monolayers in simulated body environment. Journal of Biomedical Materials Research 50, 16-20 (2000). 113. Zhai Y, Cui FZ & Wang Y. Formation of nano-hydroxyapatite on recombinant human-like collagen fibrils. Current Applied Physics 5, 429-432 (2005). 114. Sachlos E, Gotora D & Czernuszka JT. Collagen scaffolds reinforced with biomimetic composite nano-sized carbonate-substituted hydroxyapatite crystals and shaped by rapid prototyping to contain internal microchannels. Tissue Engineering 12, 2479-2487 (2006). 115. Sachlos E, Reis N, Ainsley C, Derby B & Czernuszka JT. Novel collagen scaffolds with predefined internal morphology made by solid freefrom fabrication. Biomaterials 24, 1487-1497 (2003). 116. Wahl DA, Sachlos E, Liu C & Czernuszka JT. Controlling the processing of collagen-hydroxyapatite scaffolds for bone tissue engineering. Journal of Materials Science: Materials in Medicine 18, 201-209 (2007). 117. Roveri N et al. Biologically inspired growth of hydroxyapatite nanocrystals inside self-assembled collagen fibers. Materials Science and Engineering C 23, 441-446 (2003). 118. Sionkowska A & Kozlowska J. Characterization of collagen/hydroxyapatite composite sponges as a potential bone substitute. International Journal of Biological Macromolecules 47, 483-487 (2010). 119. Jones GL et al. Primary human osteoblast culture on 3D porous collagehydroxyapatite scaffolds. Journal of Biomedical Materials Research 94A, 1244- 1250 (2010). 46 Introduction 120. Liu L, Zhang L, Ren B, Wang F & Zhang Q. Preparation and characterization of collagen-hydroxyapatite composite used for bone tissue engineering scaffold. Artificial cells, Blood Substitutes and Biotechnology 31, 435-448 (2003). 121. TenHuisen KS, Martin RI, Klimkiewicz M & Brown PW. Formation and properties of a synthetic bone composite: hydroxyapatite-collagen. Journal of Biomedical Materials Research 29, 803-810 (1995). 122. Miyamoto Y et al. Basic properties of calcium phosphate cement containing atelocollagen in its liquid or powder phases. Biomaterials 19, 707-715 (1998). 123. Tamimi F et al. Brushite-collagen composites for bone regeneration. Acta Biomaterialia 4, 1315-1321 (2008). 124. Moreau JL, Weir MD & Xu HH. Self-setting collagen-calcium phosphate bone cement: mechanical and cellular properties. Journal of Biomedical Materials Research 91A, 605-613 (2009). 125. Touny AH, Bhaduri S & Brown PW. Formation of calcium deficient HAp/collagen composites by hydrolysis of α-TCP. Journal of Materials Science: Materials in Medicine 21, 2533-2541 (2010). 126. Edelman GM. Cell adhesion molecules. Science 219, 450-457 (1983). 127. Ruoslahti E & Pierschbacher MD. Arg-Gly-Asp: A versatile cell recognition signal. Cell 44, 517-518 (1986). 128. Hughes D, Salter D, Dedhar S & Simpson R. Integrin expression in human bone. Journal of Bone Mineral Research 8, 527-533 (1993). 129. Saito T, Albelda S & Brighton C. Identification of integrin receptors on cultured human bone cells. Journal of Orthopaedic Research 12, 384-394 (1994). Chapter 1 47 130. Schneider G & Burridge K. Formation of focal adhesion by osteoblasts adhering to different substrata. Experimental Cell Research 21, 4264-4269 (1994). 131. Hynes RO. Integrins: bidirectional, allosteric signaling machines. Cell 110, 673-687 (2002). 132. Huhtala M, Heino J, Casciari D, de Lucie A & Johnson MS. Integrin evolution: insights from ascidian and teleost fish genomes. Matrix Biology 24, 83-95 (2005). 133. Riikonen T et al. α2β1 integrin is a positive regulator of collagenase (MMP-1) and collagen α1(I) gene expression. Journal of Biological Chemistry 270, 13548-13552 (1995). 134. Ivaska J et al. Integrin α2β1 mediates isoform specific activation of p38 and upregulation of collagen gene transcription by a mechanism involving the α2 cytoplasmatic tail. Journal of Cell Biology 147, 401-416 (1999). 135. Ivaska J et al. Integrin α2β1 promotes activation of protein phosphatase 2A and dephosphorylation of Akt and GSK3β. Molecular and Cellular Biology 22, 1352- 1359 (2002). 136. Knight CG et al. The collagen-binding A-domains of integrin α1β1 and α2β1 recognize the same specific amino acid sequence, GFOGER, in native (triplehelical) collagens. Journal of Biological Chemistry 275, 35-40 (2000). 137. Knight CG et al. Identification in collagen type I of an integrin α2β1-binding site containing an essential GER sequence. Journal of Biological Chemistry 273, 33287- 33294 (1998). 138. Gullberg D et al. Analysis of alpha 1 beta 1, alpha 2 beta 1 and alpha 3 beta 1 integrins in cell-collagen interactions: identification of conformation dependent alpha 1 beta 1 binding sites in collagen type I. EMBO journal 11, 3865-3873 (1992). 48 Introduction 139. White DJ, Puranen S, Johnson MS & Heino J. The collagen receptor subfamily of the integrins. International Journal of Cell Biology 36, 1405-1410 (2004). 140. Yamamoto M, Yamato M, Aoyagi M & Yamamoto K. Identification of integrins involved in cell adhesion to native and denatured type I collagens and the phenotypic transition of rabbit arterial smooth muscle cells. Experimental Cell Research 219, 249-256 (1995). 141. Davis GE. Affinity of integrins for damaged extracellular matrix: alpha V beta 3 binds to denatured collagen type I through RGD sites. Biochemical and Biophysical Research Communications 182, 1025-1031 (1992). Chapter 2 55 5555 55 The difractograms showed the peaks obtained for the diffraction and these were identified and compared with the crystallographic data of α-TCP (JCPDS-29-359) and β-TCP (JCPDS-9-169). Since the adsorption coefficient in both cases was the same, the relative amounts of the two allotropic phases was obtained through the ratio of intensities of the highest peaks. 2.3.2. Liquid phase The liquid phase was either a collagen solution or, in the control cements, accelerant solution (2.5% Na 2 HPO 4 ) or 50 mM acetic acid. 2.3.2.1. Preparation of collagen solutions Collagen was introduced as the liquid phase of the CPC. Collagen was extracted from calf pericardium, which was a process done by the group at Clínica de Hierro in Madrid, leaded by Eduardo Jorge-Herrero. The process by which the collagen was processed is briefly described. The pericardium from young calves was obtained from slaughterhouses and transported to the lab in a 0.9% saline solution. The tissue was afterwards cleaned to remove any remnants of fat. Collagen was then isolated by enzymatic digestion with porcine pepsin (EC 3.4.23.1), 2100 U/mg, in a proportion of 1 mg per gram of tissue in a formic acid solution with a final concentration of 0.5 N, introducing 10 ml per gram of tissue. After 20 hours of agitation at 4ºC, the tissue was centrifuged for 1 hour at 5000 x g in a Beckman L-70 centrifuge. The supernatant was precipitated with solid NaCl to reach a final concentration of 2.5 M, followed by 20 h of agitation at 4ºC. Subsequently, the samples were centrifuged for 1 hour at 23000 x g. The precipitate was redisolved in 0.5 N acetic acid and dialyzed against 0.1N acetic acid. Once dialyzed, the samples were lyophilized. Previous to the mixture with the CPC powder, three different pre-treatments were applied to the collagen. Solubilized collagen was named for the collagen that was completely dissolved in the solvent, which was a 50 mM acetic acid solution. In general, unless otherwise mentioned, the concentration used was 10 mg/ml. The fibrillisation is a process in which the different collagen molecules are associated, obtaining a fibrillised or self-assembled structure. The formation of collagen fibers 56 5656 56 Calcium Phosphate Cement-Collagen for Bone Regeneration involves the precipitation of the protein in an ordered form and was done by controlling the environmental conditions, such as pH, temperature and ionic strength. The process applied consisted on the initial solubilization in 50 mM acetic acid and the addition of a 0.3 M sodium hydrogenphosphate stock solution to obtain a final concentration of sodium hydrogenphosphate in the collagen solution of 20 mM. The solution was kept during 20-30 minutes at 37ºC, and was afterwards stabilized at pH 7.4 with the addition of NaOH 1 M. This method was a recompilation and modification of previous works reported in the literature 14,20,21 . The obtained collagen was fibrillised collagen. Finally, a third method was used, in which the solubilized collagen was afterwards cross-linked adding 1% vol Glutaraldehyde solution (GA, Sigma-Aldrich G400-4) in order to obtain a 0.2% vol GA in the collagen slurry. That means that when preparing 1 ml of soubilized collagen, 2 µl of the 1% GA solution were added. 2.3.2.2. Collagen characterization In order to compare the different collagen treatments, samples were prepared at a concentration of 10 mg/ml and were afterwards lyophilized (Cryodos Telstar) for 24 hours. The specimens were characterized by scanning electron microscopy (SEM, JEOL JSM-840) and scanning differential calorimetry (DSC 2920, TA Instruments). In order to prepare samples for SEM observation, after lyophilizing, samples were sputtered with gold in order to cover the surfaces of the collagen to make it conductive. Differential scanning calorimetry (DSC) is a thermoanalytical technique in which the difference in the amount of heat released by the study sample and a control can be measured against temperature. The main objective of DSC was to observe the denaturation temperature that involves an energy change. A scan over a range of temperatures was done. DSC was applied to each of the lyophilized materials and done at a heating speed of 10ºC/min from 25ºC to 150ºC (n=3). Negative values of heat evolution indicate exothermic process, whereas positive values indicate endothermic process. Chapter 2 57 5757 57 2.3.3. Characterization of the setting reaction and cohesion In the CPC preparation, the powder was added to the liquid phase, which was the collagen solution. The optimum L/P ratio was adjusted depending on the workability, ability to inject and the setting time. The L/P used in this chapter was maintained constant to 0.45 ml/g, unless otherwise specified. Three variables were studied: collagen concentration (10 and 50 mg/ml), initial powder size (coarse and fine) and collagen treatment (fibrillised or non-fibrilised, as well as cross-linked collagen in some cases). From now on, the samples will be named as a function of the concentration (10 or 50), with the designation of the initial particle size (C or F) and if it is fibrillised or not (F or blank). The samples studied and the codes used are displayed in Table 2.1. Code Particle size Collagen concentration (mg/ml) Collagen treatment CTRLC Coarse 0 N.A. COLC10 Coarse 10 Solubilized COLC10F Coarse 10 Fibrillised COLC50 Coarse 50 Solubilized COLC50F Coarse 50 Fibrillised CTRLF Fine 0 N.A. COLF10 Fine 10 Solubilized COLF10F Fine 10 Fibrillised COLF50 Fine 50 Solubilized COLF50F Fine 50 Fibrillised Table 2.1. Samples studied and codes used for this chapter. The three main variables studied were the particle size (Coarse/Fine), the collagen concentration (0, 10 and 50 mg/ml) and the collagen treatment (Solubilized/Fibrillised). 2.3.3.1. Setting and cohesion times The setting time of a CPC is the time upon which the cement starts to harden and cannot be molded anymore. When the powder is mixed with the liquid, a plastic and moldable paste is obtained. As time evolves, the paste loses its plasticity and mouldability, but increases its strength. The initial time in which a moldable paste loses its plasticity is called setting time. 58 5858 58 Calcium Phosphate Cement-Collagen for Bone Regeneration The setting time can be monitored through different methods and can take into account several properties of the CPC. It can be tracked through viscosity measurements, through the heat released in the reaction or the dissolution of the reagents, among others. The Gilmore needles are considered the easiest and fastest way to control the setting time. The protocol is described in the ASTM Standard C266-99. It is based on the resistance to the indentation of a needle on the cement. The system consists of two needles: a thick needle that has a weight of 113.4 g and a thin needle that has a weight of 453.6 g. The initial and final setting time are defined as, the time from the mixing of powder and liquid, after which the light and heavy needle did not leave any mark on the cement surface, respectively. In order to prepare the reagents to measure the setting time, the collagen was weighted, at a concentration of 10 mg/ml with a L/P ratio of 0.45. The corresponding amount of powder was weighted and mixed with the collagen solution. Once the mixing was completed, the paste was introduced in brass cylinders, 5 mm in height and 10 mm in diameter. The materials studied all had the same initial powder, being fine powder granulometry in this case, presenting different liquid solutions. The different solutions were the external control, which was an accelerant solution composed of 2.5% Na 2 HPO 4 and the internal control, which was 50 mM acetic acid solution. The collagen was mixed in the form of solubilized collagen, fibrillised collagen and crosslinked collagen. Another liquid phase used was a 0.2% GA solution. Once implanted, a CPC is going to be surrounded by the body plasma and it has to be able to stay as a whole. The cohesion time is defined as the minimum time that takes place since the initial contact of the liquid phase with the solid phase, so that the immersed paste in a liquid is maintained and does not disintegrate. In order to observe if the samples had cohesion after 2 minutes of preparation, the CPCs were mixed, being introduced afterwards in a water bath at 37ºC. The CPC prepared presented as liquid phase acetic acid, soluble collagen and fibrillised collagen. Chapter 2 59 5959 59 2.3.3.2. Differential Scanning Calorimetry Differential scanning calorimetry monitored at 37ºC was done in order to observe the energy evolution during the initial setting time. Between 50 and 100 mg of the composite were introduced in the lit, closing with the tap, without encapsulating the sample to avoid pressing the sample and pushing the water out of the capsule. In the space designated for the control in the DSC, another lit with tap was placed. The voltage needed to maintain the experimental samples and the control at the same temperature was recorded with time. The voltages were then converted to heat evolution using thermoelectric calibration constant and normalizing by the weight (W/g). The effect of collagen concentration was observed in these DSC, comparing CPC with a 10 mg/ml (COLF10 ) and a 50 mg/ml (COLF50) collagen concentration, with a cement containing acetic acid (CTRLF) in its liquid phase (n=3). Since the mixing of the liquid phase and the powder phase were done outside the DSC, the initial minutes of setting were not observed. Furthermore, since the lit was not encapsulated in order to avoid extrusion of the liquid when encapsulating, there also existed a chance that part of the liquid evaporated. According to literature, some authors covered the CPC only with parafilm, but did not cover the samples with a tap 25-28 . In those works, no effect was attributed to water evaporation. 2.3.3.3. pH evolution The pH evolution was determined of two slurries with a high L/P ratio. The L/P ratio was maintained high in order to allow the pH-meter to take the measurements. The liquid and the powder were mixed in a beaker and stirred by means of magnetical agitation. The pH-meter was then introduced in the beaker and the pH value was taken every 5 seconds. Soluble collagen was mixed with α-TCP at L/P ratios of 14.29 and 33.33 ml/g for 1 hour with a collagen concentration of 5 mg/ml (n=3). These values of L/P ratios were taken from previous literature work in order to be able to compare the results 29 . Acetic acid and water were mixed at the same L/P ratios and were used as controls (n=3). 60 6060 60 Calcium Phosphate Cement-Collagen for Bone Regeneration 2.3.4. Calcium phosphate cement properties 2.3.4.1. Collagen liberation during setting Bradford spectrophotometric analysis was done in order to determine the amount of collagen released from the CPC. For that purpose, the cement with collagen was soaked in distilled water in order to control the amount of collagen that was released from the cements during the 7 day setting reaction. The cements were prepared mixing the fine powder with two different collagen concentrations of the solubilized collagen, 10 and 50 mg/ml. The samples studied were COLF10 and COLF50, as well as the same samples with crosslinked collagen (COLF10-GA and COLF50-GA). The reason to compare the solubilized collagen with the crosslinked solublized collagen was to observe if the collagen would dissolve and would be released to the water without the crosslinking with GA. The crosslinked collagen was used as a control since it is known that with the GA crosslinking, collagen is stable and does not dissolve when put in contact with an aqueous solution. The amount of sample studied was, approximately, 0.5 grams of cement paste, meaning that the amount of collagen was 0.2 ml. That means that there were 2 mg of collagen in the whole sample in the 10 mg/ml concentration collagen CPC and 10 mg of collagen for the 50 mg/ml CPC. The samples were then introduced in two different amounts of distilled water: 1 ml and 12 ml. All the water was removed for analysis and replaced after 1, 2, 3, 4, 5, and 6 hours and then every day, up to 7 days, doing the experiment in triplicates. The Bradford protein assay was used and it is a method to determine the total protein concentration. The concentration interval in which the spectrophotometric response is linear respect to the protein concentration is the range between 1.25 and 25 µg/ml. 100 µl of the supernatant were collected and mixed with 100 µl of the Bradford reagent. It is based on the binding of the dye Coomassie to the protein. In the studied range of assay, the dependence is linear between the amount of protein present and the amount of protein linked to the dye. The assay is colorimetric, which means that the increase in color intensity increases with the protein concentration. The protein concentration was Chapter 2 61 6161 61 then determined by comparison with standard protein of bovine serum albumin solutions, measured at an absorbance of 595 nm. In order to verify and corroborate the results, a nanodrop spectrophotometer (NanoDrop 8000 Spectrophotometer, Thermo Scientific), which consists of a spectrophotometer of high accuracy that only needs 1-2 µl of sample to do the measurement, was used. This technique is useful, accurate and fast for determining nucleic acids and proteins. The different solutions were measured without any dilution. 2.3.4.2. Collagen distribution The distribution of the collagen in the cement was evaluated by fluorescence technique using (3-(4-carboxybenzoyl)quinoline-2-carboxaldehyde) (CBQCA) as fluorescent agent. This reagent has the ability to link to amino groups. A 48 well plate was used and several pieces of the set cement, which was set in water for 7 days, were introduced in them (n=3). A total volume of 600 µl was introduced in each well, containing a 1 mM solution of CBQCA (previously dissolved in acetone) and 2 mM in KCN. The samples were left reacting for 90 minutes and rinsed afterwards three times in distilled water for 15 minutes. Samples were observed by means of confocal microscopy (Leica TCSSPE), soaking them in distilled water and leaving them immersed in water during the observation in order to avoid the interference of salts. Fluorescence images at 488 nm and reflexion images were taken for each sample. Since CPC may present some autofluorescence, a CPC without collagen was used to measure the background fluorescence. Afterwards, samples were analyzed in the same conditions, making any signal of fluorescence arise from the collagen molecule. The studied samples were CTRLF, COLF10, COLF10F, COLF50 and COLF50F. 2.3.4.3. Scanning electron microscopy (SEM) The samples were freeze-dried to eliminate water, in order to facilitate gold sputtering of the samples. Once the samples were coated, the samples were observed in a SEM (JEOL JSM-840). 62 6262 62 Calcium Phosphate Cement-Collagen for Bone Regeneration 2.3.4.4. Fourier Transformed Infrared Spectroscopy The material analyzed consisted of the CPC with the different collagen treatments, in order to see the differences with a collagen concentration of 10 mg/ml and 50 mg/ml (COLF10, COLF10F, COLF50, COLF50F and CTRLF) (n=3). The methodology consisted on crashing the composite, to obtain a fine powder that was then mixed at a ratio of 1:100 with potassium bromide (KBr). Potassium bromide is transparent to the IR and does not interfere with the measure. Both of the powders were homogenously mixed and introduced in a device on top of which a load of 1000 kg.cm -2 was applied. The result was a semitransparent disk with which the measurement was done. The disk was afterwards placed in the spectrophotometer (FTIR Bomem MB-120) and the measurement was done. The spectrums were done 30 times and an average spectrum was obtained. A blank with no sample was obtained in order to have the base line. In order to observe better the possible interactions of HA and collagen, a 70:30 wt% CPC:collagen in weight composite was prepared with soluble collagen (n=3) in order to increase the amount of collagen in the composite. The collagen was prepared at a concentration of 50 mg/ml, and in order to maintain the ratio 70:30 %wt, a L/P ratio of 8.62 ml/g was used. In this case, in which the proportion of collagen was higher, the samples had sponge-like morphology, making difficult crashing the samples. Therefore, random parts of the composite were cut and placed in a diamond cell and observed with an IR Microscope Plan Spectra Tech attached to the previous FTIR, Bomem MB-120. 2.3.4.5. X-Ray diffraction X-Ray diffraction was carried out in order to determine the phase evolution from the initial stages until the end product was obtained. In this case, the process applied was the same as in section 2.3.1.2, but the comparison was done between the JCPDS cards of α-TCP and HA (JCPDS-9-432). Fine CPC composed of acetic acid (CTRLF), solubilized collagen (COLF10) and fibrillised collagen (COLF10F) as the liquid phase were prepared and left setting for 1, 2, 4, 8, 16, 24, 48, 72, 96, 120, 168, 240 and 336 hours (n=1). The amount of α-TCP Chapter 2 63 6363 63 that had reacted at time t was determined through the reaction conversion with the formula: Where w t is the fraction of α-TCP at time t, I t is the intensity of the peak 30.74º at time t, M CDHA is the adsorption coefficient of the CDHA, which is 84.97 cm 2 /g, I 0 is the intensity of the peak at time zero and M α-TCP is the adsorption coefficient of α-TCP, which is 86.43 cm 2 /g. The standard deviation was taken as the square root of the intensity 30 . 2.3.4.6. Helium pycnometry The skeletal density of a material can be calculated by introducing a determined amount of sample and measuring the volume it occupies using a Helium pycnometer (AccuPyc 1330). The pycnometer is based in two cells: the calibrated sample cell (V cell ), in which the sample is introduced and the calibrated expansion cell (V exp ). The first assumption is that V cell and V exp are at ambient pressure (P a ) and ambient temperature (T a ) and that the valve that communicates both of the cells is closed. V cell is then charged up to an elevated pressure (P g ). Since this technique is non-destructive, a total of three cylinders (∅= 6 mm and h=12 mm) before being used for the mercury intrusion porosimetry, were weighted and then introduced in the chamber. The process was repeated three times with different cylinders. 2.3.4.7. Mercury intrusion porosimetry Mercury intrusion porosimetry (MIP, Micromeritics, Autopore IV) was used to measure total porosity of the samples, as well as to obtain a pore size distribution of the sample represented as dV/dlogD respect pore entrance diameter (D). Three different variables were studied: initial powder particle size, collagen concentration and fibrillisation of collagen (n=1). 64 6464 64 Calcium Phosphate Cement-Collagen for Bone Regeneration 2.3.4.8. Injectability Injectability can be defined as the ability a paste has to be extruded through a syringe. It was measured by the weight percentage of the cement paste that was injected from a standard syringe, by a force of 100 N. A L/P ratio of 0.45 ml/g was used. Before the mixture of the two components, a 5 ml syringe with a 2 mm opening was weighted (W e ). The paste was then introduced in the syringe and weighted again (W f ). The syringe was then placed in the mechanical compression instrument (MTS Bionix 858), at an advancing speed of 15 mm/min until a 100 N force was obtained. At the end of the assay, the syringe was weighted (W a ). The injectability (I) was defined as: The assay was done for a minimum of three samples and all the samples were injected 2 minutes after mixing the powder and the liquid. The samples studied were CTRLF, COLF10 and COLF10F (n=3). 2.3.4.9. Mechanical properties Cylinders were prepared introducing the slurries into Teflon cylinder moulds of 12 mm height and 6 mm diameter and left reacting for seven days in Ringer’s solution. The CPC cylinders were then extracted from the Teflon mould and tested. A standard number of ten cylinders were prepared for each composition and used for compression testing in Universal Testing Machine (Adamel Lhomargy DY 34) at a crosshead speed of 1 mm/min. The force was axially applied. The samples analyzed were CTRLF, COLF10, COLF10F, COLF50, COLF50F, CTRLC, COLC10, COLC10F, COLC50 and COLC50F. A representation of the force applied versus the displacement was recorded. These units were given as force, in Newtons, and the displacement, in mm. The force was then transformed into stress, by dividing the force by the area and the displacement was transformed into strain, by subtracting the initial length of the material and dividing by the initial length, obtaining a dimensionless value. Calculating the stress in compression gives a negative value, since the initial value is bigger than the final value. Absolute Chapter 2 71 7171 71 Figure 2.7. Heat evolution in logarithmic scale for the setting reaction of the CPC mixed with collagen (10 mg/ml and 50 mg/ml) and acetic acid at a L/P ratio of 0.45 ml/g. 2.4.3.3. pH evolution Figure 2.11 shows the pH evolution when mixing the fine CPC powder with different solutions as liquid phase (water, 50 mM acetic acid or 10 mg/ml collagen solution in 50 mM acetic acid). The increase of the pH was similar when having water, acetic acid or the collagen solution (Figure 2.8). Nevertheless, compared to water solution, there was a delay in the dissolution kinetics. The pH plateau was achieved earlier in the water containing cements than in the collagen or acetic acid containing cements. When the L/P ratio was decreased, the acetic acid and the collagen containing mixtures continued having a delay in the dissolution kinetics. Furthermore, there was also a slight delay in the dissolution kinetics in the collagen containing samples compared to the acetic acid containing samples (Figure 2.9.). This can be observed since the collagen and acetic acid curves do not completely overlap at low times. -0,12 -0,1 -0,08 -0,06 -0,04 -0,02 0 0,01 0,1 1 10 100 1000 Heat evolution (W/g) Time (min) CTRLF COLF10 COLF50 exo 72 7272 72 Calcium Phosphate Cement-Collagen for Bone Regeneration Figure 2.8. pH curve for differente cement formulations containing water, 50 mM acetic acid solution or 5 mg/ml collagen solution in 50 mM acetic acid as the liquid phase of the CPC, at a L/P ratio of 33.33 ml/g. Figure 2.9. pH curve for differente cement formulations containing water, 50 mM acetic acid solution or 5 mg/ml collagen solution in 50 mM acetic acid as the liquid phase of the CPC, at a L/P ratio of 14.29 ml/g. 3 4 5 6 7 8 9 0 10 20 30 40 50 60 pH Time (min) L/P = 33.33 Water Acetic Ac Collagen 3 4 5 6 7 8 9 0 10 20 30 40 50 60 pH Time (min) L/P = 14.29 Water Acetic Ac Collagen Chapter 2 73 7373 73 2.4.4. Calcium phosphate cement properties 2.4.4.1. Collagen release during the setting reaction The amount of collagen released from the samples was analyzed for up to 7 days. Collagen is known to be soluble in acidic conditions and is not supposed to be soluble in neutral pH. However, in order to know if collagen was being dissolved during the soaking period in water, where the cements were immersed while the setting reaction was taking place, Bradford analysis was done. No change in the coloration of the solution was observed, neither with the cross-linked nor the non-crosslinked collagen for the different time points, meaning that the amount of collagen released in the medium at the different time points, if any, was very low, below the detection limit. From these results, it can be concluded that the amount of collagen dissolved was lower than 1.25 µg/ml in the different amounts of water, both for the crosslinked and the noncrosslinked specimens for the different time points, which would represent less than a 0.025% of collagen dissolved to the medium when having a 10 mg/ml collagen concentration in the 1 ml sample. In the 10 mg/ml collagen CPC immersed in 12 ml, the release was lower than 0.3% collagen. Furthermore, for the 50 mg/ml solution immersed in the 1 ml and 12 ml, the maximums released were lower than 0.005% and 0.06% respectively. From these results, it was concluded that collagen crosslinking was not necessary. The same result was obtained from the Nanodrop spectrophotometer, in which the concentration of the protein detected didn’t differ from the blank. The different values oscillated around 0. The detection limit of the spectrophotometer was 0.0025 mg/ml. 2.4.4.2. Collagen distribution CPC presented autofluorescence when observed under confocal microscopy. Therefore, the intensity that was observed for the CTRLF was substracted for all other samples. The first samples analyzed were the samples COLF10 and COLF50 (Figure 2.10). The image in the left corresponds to the reflection image and the image in the right 74 7474 74 Calcium Phosphate Cement-Collagen for Bone Regeneration corresponds to the image taken with the exciting laser beam. For COLF10 (Figure 2.10b), the intensity was lower compared to COLF50 (Figure 2.10d). In both cases, the distribution was shown to be homogenous; the only thing that varied was the intensity, which was dependent on the concentration. Figure 2.10. Distribution of collagen in a cement with L/P of 0.45 ml/g with solubilized collagen at two different concentrations after 7 day immersion in water: 10 mg/ml (a,b) and 50 mg/ml (c,d). a) corresponds to the optical image of the studied area of the cement for the 10 mg/ml solubilized collagen, b) corresponds to the fluorescence image of the studied area of the cement for the 10 mg/ml solubilized collagen, c) corresponds to the optical image of the studied area of the cement for the 50 mg/ml solubilized collagen, d) corresponds to the fluorescence image of the studied area of the cement for the 50 mg/ml solubilized collagen. Regarding the fibrillised collagen, the structure was completely different (Figure 2.11). There were areas in which the collagen was present, and parts of the CPC in which no collagen was present at all. When collagen was fibrillised, a non-homogenous a b c d Chapter 2 75 7575 75 distribution was observed, although an increase of the intensity in the areas in which collagen was present, compared to the COLF10 and COLF50, was observed. The difference when comparing low concentration with a high concentration was the higher amount of gaps that the COLF10F left (Figure 2.11b). For COLF50F, collagen appeared almost in the totality of the sample (Figure 2.11d.), whereas for COLF10F, collagen only appeared in some parts. The intensity was higher in both cases compared to the same concentrations with the solubilized collagen. Figure 2.11. Distribution of collagen in a cement with L/P of 0.45 ml/g with fibrillised collagen at two different concentrations after 7 day immersion in water: 10 mg/ml (a,b) and 50 mg/ml (c,d). a) corresponds to the optical image of the studied area of the cement for the 10 mg/ml fibrillised collagen, b) corresponds to the fluorescence image of the studied area of the cement for the 10 mg/ml fibrillised collagen, c) corresponds to the optical image of the studied area of the cement for the 50 mg/ml fibrillised collagen, d) corresponds to the fluorescence image of the studied area of the cement for the 50 mg/ml fibrillised collage. a b c d 76 7676 76 Calcium Phosphate Cement-Collagen for Bone Regeneration In summary, the collagen distribution was homogenous for soluble collagen, whereas in tended to be heterogeneous for fibrillised collagen. As the amount of collagen was increased, the intensity also increased for the soluble collagen, and not so much for the fibrillised collagen. 2.4.4.3. Scanning electron microscopy As can be seen in Figure 2.12a, the fracture surface images of CTRLF revealed that HA crystals were aggregated surrounding the original α-TCP particles. Typical Hadley cells were observed, showing an empty thick shell of hydration products inside which a α- TCP grain had fully reacted. At higher magnifications, it was seen that the structure consisted of a network of small HA crystals, combined with some bigger crystals (Figure 2.12b). Regarding COLF10, the morphology was similar to that of CTRLF (Figure 2.12c and d). The presence of the collagen was not detected with this type of technique. In contrast, the collagen was observed in the samples containing fibrillised collagen (Figure 2.12e and f). In this case, the collagen was observed as bundles of collagen fibers arranged on top of the CPC crystals. These fibers were only observed in some parts of the CPC composite. The morphology was similar between the fibrillised collagen and crosslinked collagen with GA (Figure 2.12g and h). Chapter 2 77 7777 77 Figure 2.12. SEM micrographs for the different CPC materials at two different magnifications for a L/P ratio of 0.45 ml/g after 7 day immersion in Ringer solution: a) and b) CTRLF, c) and d) COLF10, e) and f) COLF10F, g) and h) COLF10 crosslinked with GA. a b d g h c e f 78 7878 78 Calcium Phosphate Cement-Collagen for Bone Regeneration 2.4.4.4. Fourier Transformed Infrared Spectroscopy Figure 2.13 shows the results for the fine CPC for the two different concentrations and the two different collagen treatments (solubilized and fibrillised) after 7 days of setting in Ringer´s solution at 37ºC. Attention should be focused on the amide I region, which is located in the 1658 cm -1 zone. This gives information on the C=O bond of the carboxylic acid in the collagen and the possible interaction with the calcium phosphate. As can be seen, the information given by Figure 2.13 is quite limited in this respect, since a very small band appears in this area and no shifts can be observed. This band also appears in the CTRLF, meaning that the band arises from the CPC and not from the collagen. The main band observed is the phosphate band at 1026 cm -1 , which corresponds to the stretching of the PO 43- group in the HA. Figure 2.13. FTIR spectrum for the different materials at L/P ratio of 0.45 ml/g after 7 day immersion in Ringer solution for: CTRLF, COLF10, COLF10F, COLF50 and COLF50F. The assignment of the different bands represented in Figure 2.13 is summarized in Table 2.3. -0,5 0,5 1,5 2,5 3,5 4,5 5,5 800 1300 1800 2300 2800 3300 3800 Absorbance (AU) Wavenumber (cm-1) COLF50F COLF50 COLF10F COLF10 CTRLF 3415 3521 1620 1210 1130 1085 1026 1006 844 Chapter 2 79 7979 79 Wavenumber (cm-1) Vibration 3521 OH stretching 3415 Water-adsorbed deformation 1620 OH water-adsorbed bending 1210 δ OH mode of HPO 4 2 - hydrogenbonded 1130 ν 3 vibration component of HPO 4 2- groups 1085 ν 3 (PO4) 1026 ν 3 (PO4) 1006 ν 1 (PO4) 844 ν 3 P-O(H) deformation of HPO 4 2- groups Table 2.3. Main FTIR bands observed for the CPC at a L/P ratio of 0.45 ml/g after 7 day immersion in Ringers solution. The same bands were observed for all the studied materials: CTRLF, COLF10, COLF10F, COLF50 and COLF50F. In order to verify what kind of interaction appeared between the collagen and the cement, and taking into account that the amount of collagen used in the prepared cements were too low for IR detection, the amount of collagen was increased. A CPC containing a 50 mg/ml collagen solution at a L/P ratio of 8.62 ml/g, which corresponded to a 70/30 % w/w composite of cement/collagen was prepared. Figure 2.14 shows the main bands observed in it with the corresponding assignation. Figure 2.14. FTIR spectrum of the a composite prepared in the ratio in weight 30:70 of collagen:CPC after 7 days in aqueous solution, compared to the CPC for 7 days in aqueous solution and collagen. 0 0,5 1 1,5 2 2,5 750 950 1150 1350 1550 1750 1950 Absorbance (AU) Wavenumber (cm-1) CPC 70:30 wt% CPC:collagen Collagen Amide I Amide I I Amide I II PO 4 3 - band HPO 4 2 - - CO O - C - N CO 3 2 - 80 8080 80 Calcium Phosphate Cement-Collagen for Bone Regeneration In this case, the main shifts observed were in the phosphate band, which did not exist in collagen, which appeared at 1031 cm -1 for calcium phosphate and changed to 1024 cm -1 for the composite material (Figure 2.15). There are two other bands which also correspond to the phosphate group that appeared at 961 cm -1 for the CDHA and the composite, and another band at 1111 cm -1 , that also had the same value for the composite. The shoulder at 1145 cm -1 only appeared on the CPC. The other band present that appeared at 872 cm -1 corresponded to the presence of the hydrogenphosphate group. Figure 2.15. FTIR spectrum of the CPC, composite material made of 70:30 %wt CPC:collagen and collagen. The L/P ratio used for the CPC was 8.62 ml/g and was then left in water for 7 days for the complete transformation into CDHA. The presented area corresponds to the phosphate modes of vibration. Only one shift appears which corresponds to the phosphate mode of vibration 3. The dotted line indicates the presence of a shift. The assignment of the different bands observed in Figure 2.15 is shown in Table 2.4. CDHA band (cm - 1 ) Composite band (cm - 1 ) Assignment 1145 - ν 3 vibration component of HPO 4 2 - groups 1111 1111 υ 3 (PO4) 1031 1024 ν 3 (PO4) 961 961 ν 1 (PO4) 872 872 ν 3 P-O(H) deformation of HPO 4 2 - groups 0 0,5 1 1,5 2 2,5 800 850 900 950 1000 1050 1100 1150 1200 Absorbance (AU) Wavenumber (cm-1) CPC 70:30 wt% CPC:collagen Collagen υ 3 PO 4 3 - υ 1 PO 4 3 - HPO 4 2 - Table 2.4. FTIR bands and assignation of the phosphate zone of the composite material made of 70:30 %wt CPC:collagen and the CPC. The L/P ratio used was 8.62 ml/g and the samples were then left in water for 7 days for the complete transformation into CDHA. Chapter 2 87 8787 87 incorporated. The values decreased from 2.86 g/cm 3 for the CTRLF, to 2.84 g/cm 3 for the 10 ml/mg collagen containing CPC and up to 2.80 g/cm 3 for the 50 ml/mg collagencontaining CPC. The relationship was inversely proportional to the concentration, meaning that as the collagen concentration increased, the density decreased. There were no significant differences when comparing the fibrillised collagen samples and the nonfibrillised collagen samples. Figure 2.22. Skeletal density for the CPC with fine initial particle size with and without collagen for a L/P ratio of 0.45 ml/g. 2.4.4.7. Porosimetry The total porosity of the samples and the pore size range measured by MIP are shown in Table 2.6. The porosities for the different samples were shown to range between 41% and 48%. The measured pore size ranged between 0.006 µm for the lowest limit, since it is the limit of detection of the porosimeter, and 4.7 µm. Nevertheless, the peak of the different pore size distributions was in the same order of magnitude for the different samples. 2,74 2,76 2,78 2,8 2,82 2,84 2,86 2,88 CTRLF COLF10 COLF10F COLF50 COLF50F Density (g/cm3) 88 8888 88 Calcium Phosphate Cement-Collagen for Bone Regeneration POROSITY (%) RANGE (µ µµ µm) Ma in peak (µm) Secondary peak (µm) CTRLC 41,2 0,006-1,312 0.021 0.0770 COLC10 41,1 0,006-1,412 0.095 - COLC10F 47,3 0,006-2,664 0.032 0.730 COLC50 43,9 0,006-0,121 0.040 - COLC50F 43,6 0,006-3,142 0.095 - CTRLF 42,9 0,006-0,121 0.017 - COLF10 43,1 0,006-0,520 0.017 - COLF10F 44,1 0,006-0,329 0.021 - COLF50 41,2 0,006-0,095 0.014 - COLF50F 48,0 0,006-4,707 0.026 0.403 Table 2.6. Values for the total porosity, pore size range and highest volume pore sizes for the materials composed of CPC with and without collagen as the liquid phase of the CPC for a L/P ratio of 0.45 ml/g. The information shown in Table 2.6 was extracted from Figure 2.23 to Figure 2.28 that represent the entrance pore size distribution for the different samples. Figure 2.23. Pore size distribution for CTRLF and CTRLC for a L/P ratio of 0.45 ml/g using 50 mM acetic acid as liquid phase. It can be seen that the coarse CPC had a pore size distribution between 0.006 µm and 1 µm, whereas the fine CPC had a narrower pore size distribution which ranged between 0.006 µm and 0.1 µm (Figure 2.23). The total porosity of the samples was similar, with a value of 41% for the CTRLC and 43% for the CTRLF. 0 0,1 0,2 0,3 0,4 0,5 0,6 0,001 0,01 0,1 1 10 100 1000 dV/dlogD Pore size (µ µµ µm) control F control c CTRLF CTRLC Chapter 2 89  The pore size distribution of the samples containing solubilized collagen is shown in Figure 2.24. In the COLF10 and COLC10 samples, the results were very similar to those for their respective controls (Figure 2.24a). When the collagen was incorporated in higher concentrations (COLF50 and COLC50), there was a small shift to lower pore sizes in both cases (Figure 2.24b). The peak became narrower, and for the COLC50, the pore size was reduced to 0.1 µm. Figure 2.24. Pore size distribution comparing the two different CPC initial particle size distributions in the presence of collagen: COLF and COLC for two different concentrations at a L/P ratio of 0.45 ml/g: a) 10 mg/ml and b) 50 mg/ml. The results for the samples containing fibrillised collagen are shown in Figure 2.25. For the low concentration (COLF10F and COLC10F), the pore size distribution was similar to the control (CTRLF and CTRLC) and for COLC10F, there were a higher number of pores in the submicron range, which was associated with a slight increase in the total porosity (47% for COLC10F and 41% for CTRLC) (Figure 2.25.a). As observed in Figure 2.25b, when the collagen was incorporated in higher concentrations, COLC50F had similar pore size distribution and porosity to the CTRLC, whereas COLF50F had a higher total porosity (48%) than the CTRLF (43%) associated with an increase in the micron sized pores volume. 0 0,1 0,2 0,3 0,4 0,5 0,001 0,1 10 1000 dV/dlogD Poresize(m) COLF10 colc10 COLF10 COLC10 0 0,2 0,4 0,6 0,8 1 0,001 0,1 10 1000 dV/dlogD Poresize(m) COLF50 colc50 a bCOLF50 COLC50 0 0,1 0,2 0,3 0,4 0,5 0,001 0,1 10 1000 dV/dlogD Poresize(m) COLF50F colc50f COLC50F 0 0,1 0,2 0,3 0,4 0,5 0,6 0,001 0,1 10 1000 dV/dlogD Poresize(m) COLF10F colc10f a b COLC10F Figure 2.25. Pore size distribution comparing the two different CPC initial particle size distributions in the presence of fibrillised collagen: COLF and COLC for two different concentrations at a L/P ratio of 0.45 ml/g: a) 10 mg/ml and b) 50 mg/ml. 90 9090 90 Calcium Phosphate Cement-Collagen for Bone Regeneration The comparison between the solubilized and the fibrillised collagen in the samples with 10 mg/ml and 50 mg/ml can be found in Figure 2.26. The curves for the coarse CPC were very similar among them (Figure 2.26a), as well as the curves for the fine CPC (Figure 2.26b), which were also very similar among them. That means that there is no direct effect of the presence of soluble collagen or fibrillised collagen at low collagen concentrations on the pore size distribution. Figure 2.26. Pore size distribution comparing the soluble collagen and the fibrillised collagen composite with the control at 10 mg/ml for at a L/P ratio of 0.45 ml/g: a) coarse and b) fine. In order to see the effect at higher concentrations of collagen, the same parameters were compared with the high collagen concentration, 50 mg/ml (Figure 2.27.). Regarding coarse CPC, the COLC50F and the CTRLC were very similar, whereas the COLC50 had a much narrower distribution. Regarding the fine CPC, CTRLF and COLF50 had similar distributions, whereas the COLF50F was the one with a broader distribution. Figure 2.27. Pore size distribution comparing the soluble collagen and the fibrillised collagen composite with the control at 50 mg/ml for at a L/P ratio of 0.45 ml/g: a) coarse and b) fine. 0 0,05 0,1 0,15 0,2 0,25 0,3 0,35 0,001 0,1 10 1000 dV/dlogD Pore size (µm) CTRLC COLC10 COLC10F 0 0,1 0,2 0,3 0,4 0,5 0,6 0,001 0,1 10 1000 dV/dlogD Pore size (µ µµ µm) CTRLF COLF10 COLF10F 0 0,2 0,4 0,6 0,8 1 0,001 0,1 10 1000 dV/dlogD Pore size (µm) CTRLC COLC50 COLC50F 0 0,2 0,4 0,6 0,8 1 0,001 0,1 10 1000 dV/dlogD Pore size (µ µµ µm) CTRLF COLF50 COLF50F a b b a Chapter 2 91 9191 91 Finally, in order to compare different concentrations, the samples with the two concentrations were compared among them with their respective controls (Figure 2.28.). For the coarse CPC, as was previously seen, the 10 mg/ml had no effect on the pore size distribution, whereas the 50 mg/ml reduced the peak to 0.1 µm. Regarding fine CPC, COLF10 did have a small increase in the pore size distribution compared to CTRLF, whereas COLF50 decreased the pore size distribution compared to CTRLF. Figure 2.28. Pore size distribution comparing the two collagen concentrations (10 and 50 mg/ml) with the control for a determined initial CPC particle size for a L/P ratio of 0.45 ml/g, being a) coarse and b) fine. 2.4.4.8. Injectability Figure 2.29 shows the injectability of the control cement and the collagen-containing cements. For the CTRLF, 50% of the paste was injected, whereas for COLF10 and COLF10F, 96% and 65% of the paste were injected, respectively. 0 0,2 0,4 0,6 0,8 1 0,001 0,1 10 1000 dV/dlogD Pore Size (µm) CTRLC COLC10 COLC50 0 0,2 0,4 0,6 0,8 1 0,001 0,1 10 1000 dV/dloD Pore size (µ µµ µm) CTRLF COLF10 COLF50 0 20 40 60 80 100 120 CTRL COLF10 COLF10F Injectability (%) b a Figure 2.29. Percentage of injectability for CTRLF, COLF10 and COLF10F for L/P ratio of 0.45 ml/g. 92 9292 92 Calcium Phosphate Cement-Collagen for Bone Regeneration The force diagram is shown in Figure 2.30. Regarding CTRLF, it was seen that the force started increasing as the piston slowly advanced. Every time the piston advanced, the force increased and it was more difficult to inject the paste. A different behavior was observed for the soluble and fibrillised collagen (COLF10), in which the force increased up to 20 N, and at that force, a plateau was reached. The plateau was maintained until the force started to increase in the case of the COLF10F, not being able to inject all the paste. However, for COLF10, the force remained constant at the 20 N value until all the paste was completely injected. The force increased to 100 N when the piston reached the end of the syringe. Figure 2.30. Force diagram for the injected materials CTRLF, COLF10 and COLF10F for L/P ratio of 0.45 ml/g. Figure 2.31 shows the initial yield force needed to start injecting the paste. It can be seen that the CTRLF and the COLF10 had similar values, being 21.5 ± 1.5 N and 20.6 ± 1.7 N respectively. The yield force for COLF10F was higher, 25.1 ± 0.5 N. Furthermore, it is also interesting to note that in both of the cases in which collagen was present, once the paste started to be injected, the force started to increase. Afterwards, a considerable decrease in the force (5 N at the most) was observed, being able to inject the paste at the same force as the initial value. This decrease in the force was not found for the CTRLF. 0 10 20 30 40 50 60 70 80 90 100 0 5 10 15 20 25 30 Force (N) Displacement (mm) CTRLF COLF10 COLF10F Chapter 2 93 9393 93 Figure 2.31. Force diagram for the injected materials CTRLF, COLF10 and COLF10F at short displacements for L/P ratio of 0.45 ml/g. 2.4.4.9. Mechanical properties The compressive strength for the coarse and fine CPC with collagen is shown in Figure 2.32. When the collagen concentration was low (e.g. 10 mg/ml), the compressive strength of the CPC did not significantly vary. Nevertheless, when higher concentrations of collagen were incorporated in the CPC (50 mg/ml), the compressive strength of the CPC diminished. Compared to control, the samples with a concentration of 50 mg/ml of collagen presented half the compressive strength of the control material. When collagen was incorporated as fibrillised collagen, the samples presented lower values compared to those of the solubilized collagen, except for the COLF10F, in which an increase was observed, although it was not statistically significant. Significant differences were found between COLC10 and COLC10F. In general, the values obtained with the coarse CPC were lower than those with fine CPC, being the differences statistically significant for the samples CTRL, COL10F and COL50. 0 5 10 15 20 25 30 35 40 0 0,5 1 1,5 2 2,5 3 Force (N) Displacement (mm) CTRLF COLF10 COLF10F 94 9494 94 Calcium Phosphate Cement-Collagen for Bone Regeneration Figure 2.32. Maximum strength for the CPC with fine and coarse initial particle size prepared at a L/P ratio of 0.45 ml/g using acetic acid, solubilized collagen and fibrillised collagen as liquid phase of the CPC after 7 day reaction in water.*denotes significant differences between coarse and fine CPC. **denotes significant difference between the fibrillised and solubilized collagen for coarse CPC for a concentration of 10 ml/mg. Representative stress-strain curves for the different fine CPC series are shown in Figure 2.33. These curves were used to calculate the compressive strength, as well as the strain the materials presented. It is shown that the slopes of the different curves are similar to CTRLF, except for the COLF50F and COLF10F. It can be seen that the strain before breaking is higher for the fibrillised collagen composites (COLF10F and COLF50F). 0 5 10 15 20 25 30 35 40 CTRL COL10 COL10F COL50 COL50F Compressive strength (MPa) Fine Coarse 0 5 10 15 20 25 30 35 40 -2 0 2 4 6 8 10 Stress (MPa) Strain (%) CTRLF COLF10 COLF10F COLF50 COLF50F ** * * * Figure 2.33.Stress-strain curves for the fine series CPC at a L/P ratio of 0.45 ml/g after 7 days setting in water. Chapter 2 95 9595 95 2.5. Discussion 2.5.1. Collagen processing One of the objectives of the study was to characterize the effect of different collagen pre-treatments previous to the mixture with the CPC powder. That is why it was important to initially characterize the fibrillised collagen and the crosslinked collagen, compared to the solubilized collagen. The assembly of collagen molecules into fibrils is an entropy-driven process, similar to that occurring in other protein self-assembly systems, such as microtubules, actin filaments and flagella. These processes are driven by the loss of solvent molecules from the surface protein molecules and results in assemblies with a circular cross-section, which minimize the surface area/volume ratio of the final assembly. 19 The resulting molecule is rod-like and self-assembles spontaneously to form fibrils, in the process named as fibrillogensis 31,32 . The length and diameter of the fibrils will depend upon the conditions involved in the growth. The kinetics of fibrillogenesis has been previously studied. Gross was one of the first scientists to focus in collagen fibrillogenesis and made a first analysis on precipitation of collagen fibrils from neutral salts and measured the increase in opacity of the system as time evolved 13,33 . The rate of precipitation varied with temperature and ionic strength, obtaining considerable changes in the fibrils size. The variation of rate of precipitation with ionic strength and pH indicated that it was controlled to some extent by electrostatic interactions between the soluble collagen particles. 14 Collagen selfassembly involved a phase transition with no change in molecular conformation 15 . Under typical assembly conditions, which are those used in this study, which is a temperature between 31-38ºC and pH around 7, it has been reported that the intensity of scattered light measured by light scattering technique and by turbidimetric methods has a sigmoideal shape, with an initial lag phase 14,34 . The images shown by AFM in the work by Goh et al showed that at the beginning monomers, dimers and short oligomers were present. Once the lag phase concluded, the microfibrils proliferated and were present until the termination of assembly 21 . 96 9696 96 Calcium Phosphate Cement-Collagen for Bone Regeneration The process of fibrillisation was assessed in this study by DSC. It was observed that the denaturation temperature was 70ºC for the solubilized collagen, 85ºC for the crosslinked collagen and 89ºC for the fibrillised collagen (Figure 2.5). The denaturation temperature for collagen depends on the collagen source 35 . Parameters such as type of animal and tissue of origin play a key role on the final denaturation temperature, which range between 50 and 80ºC 35 , although in some animals these values can drop even more, like in the case of fishes, where the denaturation temperature is usually around 30ºC 36,37 . Concerning pericardium collagen, which was the collagen used in the present work, the denaturation temperatures were found to be around 70ºC for samples from sheep origin 38 . A study that used bovine pericardium collagen, which has the same animal origin as in the present study, reported a denaturation temperature of 70ºC 39 . This value matches exactly our values found for the solubilized collagen sample. In order to increase the denaturation temperature, which is directly related with higher mechanical properties and less degradation susceptibility, the collagen was crosslinked 40 . The method used to cross-link may affect the final denaturation temperature 41-43 . Most of the works use GA or a mixture of 1-Ethyl-3-(3- dimethylaminopropy)carbodiimide hydrochloride (EDC) and N-hydroxysulfo succinimide (NHS) for crosslinking or as controls to compare with new crosslinking methods, since they are considered the most efficient crosslinkers and present significant increase in denaturation temperature 44 . In general, the temperatures that have been reported for crosslinked pericardium collagen are similar to those presented in the present work. For instance, a temperature raise from 70ºC for the soluble collagen to 83ºC for the collagen crosslinked with Hexamethylene diisocyanate (HMDC) for bovine pericardium derived collagen was reported 39 . In two other works, the values raised up to 85ºC for the crosslinked pericardium collagen 45,46 . In another study, the crosslinking process was optimized for the NHS:EDC molecule and it was seen that the highest denaturation temperature that was obtained for bovine pericardium collagen was 86.9ºC 43 . Therefore, these values match very close the 85ºC found for our crosslinked collagen. Regarding the fibrillised collagen, up to our knowledge, no works have been reported on bovine pericardium collagen. Fibril formation involves the aggregation and alignment of collagen molecules 17,18 , which, according to previous reports, improves Chapter 2 103 103103 103 the samples were observed to be heterogeneous (Figure 2.11). The collagen bundled-up together by means of fibrillisation, making interconnections between the different collagen monomers. The light was brighter than for the solubilized collagen, because there was higher amount of collagen concentrated in certain points. Furthermore, the images also revealed that, even though the pH rises to near neutral pH when the setting reaction takes place as observed in Figure 2.8 and 2.9, and it is known that this is near the pH at which fibrillisation takes place, the collagen was still maintained as solubilized and did not fibrillise. Therefore, it was concluded that no collagen was released and that the crosslinking was not necessary. There are two reasons that explain this behavior. The first one is that the calcium phosphate is found as the matrix of the material, having the collagen between the ceramic particles. Therefore, the collagen is entrapped between the compact structures formed by the CDHA. Furthermore, since CDHA presents high amount of Ca 2+ , and collagen presents high amount of carboxylic groups, it is possible to have a chemical interaction between the two chemical groups. Similar results have been found for CPC, in which it was observed that the presence of collagen made a compact structure which did not allow for collagen to be released 22 . In general, CPC with collagen don’t incorporate crosslinkers, although no published data demonstrates the reason why it is not necessary 22,24,77 . 2.5.4. Microstructure The microstructure formed for the CPC in the presence of collagen was very similar to that of the control CPC (Figure 2.12 a-d). At low magnification, Hadley shells are visible in the structure for the CTRLF and COLF10, which are formed when α-TCP is brought in contact with water, dissolving and followed by the precipitation of CDHA surrounding the α-TCP powder, giving rise to shell-like structure (Figure 2.12 a,c). At higher magnification it was seen that the structure was conformed of an entangled network of the CDHA crystals (Figure 2.12 b). The same structure was found in the presence of solubilized collagen (Figure 2.12d). Tamimi et al observed similar microstructure both in the presence and absence of the collagen to the results observed in the present study 22 . They attributed this observation to an homogenous distribution of the collagen, and since the collagen was in the form of small molecules, it was not 104 104104 104 Calcium Phosphate Cement-Collagen for Bone Regeneration detectable by SEM 22 . This is in agreement with the fluorescence results found in the present work, in which collagen was found to be distributed homogenously. The presence of collagen was detected by SEM when the collagen was fibrillised and crosslinked (Figure 2.12 e-h), presented as bundles or membranes covering the CDHA crystals. This happened because the aggregation of the small monomers into bigger sized collagen molecules in the form of bundles, which were detectable with SEM. Moreau et al used a TTCP CPC with collagen in the form of fibers, which were clearly detectable by SEM 24 , and attributed this observation to the aggregation of different collagen molecules to form a braided structure. 2.5.5. Phase evolution and CPC-collagen interaction The XRD difractograms confirmed that the presence of collagen did not alter the setting reaction of the CPC and that CDHA was formed as the final product of the setting reaction (Figure 2.17, 2.18 and 2.19). It was also seen that the kinetics of the CDHA formation were similar in the presence of acetic acid, solubilized collagen and fibrillised collagen (Figure 2.20 and 2.21). Although in the setting reaction studies (pH evolution, DSC and Gilmore needles) a small delay was observed at very short times (during the first minutes of reaction) this does not contradict the XRD study where the first value of the kinetic study is 1 hour. In previous studies it was shown that collagen hindered the transformation of the CPC into HA also at short times 23 . Therefore, it can be concluded that a small delay is found only during the initial minutes of reaction, but after 1 hour, the conversion of the α-TCP into CDHA takes place at a similar rate in the presence and absence of collagen. The collagen molecule has about 1000 residues per chain, in which about 20 % of these residues have a side chain of COOH or NH 2 . When collagen is mixed with a calcium phosphate, the dissolution of the calcium phosphate will lead to the liberation of Ca 2+ and PO 43- ions to the medium which will be able to interact with the COO - and NH 3+ groups of the collagen molecules. These interactions, mainly electrostatic, have been previously studied by FTIR and have appeared as shifts in wavenumber when calcium and phosphate solutions were mixed with collagen solutions 78 . The interaction between the collagen and CPC for the samples with L/P ratio of 0.45 ml/g containing 10 mg/ml or 50 mg/ml solution showed no significant bands in the Chapter 2 105 105105 105 amide region (Figure 2.13). Therefore, a composite with higher content of collagen was fabricated. It was seen in the results that there were two main regions in which a shift was detected for the 70:30 wt% composite (Figure 2.14): the amide I (∼1650 cm -1 ) and amide II (∼1550 cm -1 ) region corresponding to collagen, and the ν 3 PO 43- mode of vibration (∼1030 cm -1 ) region corresponding to the CDHA. Regarding the phosphate groups, the most predominant band corresponded to the 1041 cm -1 band for the CDHA which shifted to 1031 cm -1 for the composite material (Figure 2.15, Table 2.4). A possible explanation was the interaction between the NH 3+ groups and the PO 43- groups, weakening the bond and creating the shift. Nevertheless, this shift has not been previously discussed in the literature by other authors and therefore it is difficult to speculate about the rationale behind. The most relevant bands appeared in the amide region, and more specifically, the amide I region (Figure 2.16, Table 2.5). The amide I corresponds to the bending of the bond between carbon and oxygen of the carboxylic group (C=O). It was seen that there was a shift from 1653 cm -1 for collagen to 1647 cm -1 for the composite (Figure 2.16). The observed shift was 6 cm -1 . The possible interaction present here was between the calcium atoms and the carboxylic group. These shifts have been previously discussed and will therefore be taken into consideration. The interaction in separate of collagen and Ca 2+ ions and phosphate ions can be monitored and were indeed studied in previous works. An experimental study was done in which recombinant human like collagen (RHLC) was mixed with several solutions 79 . A comparison between RHLC, RHLC with Ca ions, RHLC with phosphate ions and RHLC with calcium phosphate was done in order to see which of the ions had the biggest effect in the IR shifts. The positions of RHLC and RHLC with phosphate ions were almost the same, revealing that there was no obvious interaction between RHLC and phosphate ions. When RHLC and RHLC with Ca ions were compared, there were some differences. Two concentrations of Ca ions were introduced, for the lower concentration, amide I, appeared at 1639 cm -1 , while for the higher concentration, the amide I appeared at 1633 cm -1 . The amide I in pure RHLC was observed at 1662 cm -1 79 . When the RHLC was combined with the calcium phosphate, a similar shift appeared as the one observed when RHLC was mixed with the calcium ions, decreasing from 1662 106 106106 106 Calcium Phosphate Cement-Collagen for Bone Regeneration cm -1 for collagen to 1653 cm -1 for the composite. From these results, it can was seen that, in the mineralization of the RHLC, there is no interaction with phosphates. The red shift observed in the amide I was attributed to the weakening of the C=O bond in the peptide chain because of the formation of new chelate bonds between calcium ions and C=O bonds. This is thought to be quite reasonable since the fact that the oxygen from the carbonyl has a nonbonding pair of electrons which can chelate metal atoms 79 . This theory has been supported by other authors 4,68,79-81,92 . This was also demonstrated by a decrease in the carboxylic group bond order (from 1.76 to 1.51), meaning that the free electrons in the oxygen were able to chelate calcium ions 68 . Table 2.7 reports the values given by other authors for the wavenumbers shift in the amide I region when a calcium phosphate is incorporated in the structure of collagen. The explanation given by the different authors on the shift is the chelation of the calcium ions with the carboxylic groups of the collagen as previously explained. As can be seen in Table 2.7, the shifts are in the range of 3 cm -1 to 14 cm -1 . The range found in the present study falls within this range (6 cm -1 ). This shift can therefore be assigned to the interaction of the collagen and the CDHA. This shift and the fact of having an electrostatic binding between the collagen and the CDHA, may also be related with the fluorescent images (Figure 2.10 and 2.11). It is possible that besides the physical interaction of the collagen and the CDHA which retains the collagen in the CDHA network, there may also be a physical-chemical interaction which enhances the retention of the collagen in the structure as was shown by fluorescence. Table 2.7. Wavenumber appeared in the literature when comparing collagen and a composite composed of hydroxyapatite and collagen. 2.5.6. Density and porosity The skeletal density of composite CPC decreased as the collagen concentration was increased (Figure 2.22). Even though the presence of collagen was low, the skeletal Material Amide I shift (collagen to collagen/CaP) Author Mineralization on PHBV/collagen composite 1659 to 1656 (3 cm-1) Jingjun W 79 Collagen mineralization 1657 to 1651 (6 cm-1) Zhang W 80 Simultaneous precipitation of collagen Shift (no value given) Keeney M 81 Mineralization of recombinant human like collagen 1662 to 1653 (9 cm-1) Wang Y 92 Collagen mineralization in SBF 1663 to 1649 (14 cm-1) Zhang LJ 7 5 CPC with collagen 1653 to 1647 (6 cm - 1 ) Present study Chapter 2 107 107107 107 density decreased and this was because the collagen has a lower density than the calcium phosphate, making the material decrease its density. This skeletal density is an intrinsic property of the material. The extrinsic parameter that relates directly with the morphology of the material is the porosity. The total porosity was measured with the mercury intrusion porosimeter. The effect of three variables in the porosity of CPC were studied, being the initial particle size distribution of the powder, the presence of solubilized collagen and fibrillised collagen and the collagen concentration. The initial particle size of the cement powder, being coarse and fine, influenced the pore size range, which were higher for the coarse cements, although presented similar values of total porosity (Table 2.6). The particle size distribution was considered as the parameter that changed the most the pore sizes. Solubilized collagen was not shown to affect significantly the porosities nor the pore size distributions for the low (10 mg/ml) and high (50 mg/ml) collagen concentrations. Similar trend was observed for the fibrillised collagen at low collagen concentrations, although at higher concentrations, the presence of fibrillised collagen increased the pore size distribution to higher pore sizes. This was probably due to the fact that, as was seen in the collagen distribution observed by fluorescence, the collagen was heterogeneously dispersed, forming bundles. Once these bundles were dried, they could leave a void in which the mercury could easily penetrate and that was why these higher pore sizes were observed. It is known that porosity has high significance in the field of drug delivery systems. In fact, several studies proved the efficiency of the CPC as drug delivery vehicle 82 . The main difference of the CPC with other materials, is that the drug can be mixed with the liquid or the solid 83 , or can be incorporated by adsorption in the set cement 84 . In both of the cases, one of the most important parameters is the pore size and its pore size distribution 85,86 . In a previous study, it was shown the importance of the nano and microporosity in the CPC 87 . The influence of the initial liquid to powder ratio, as well as the influence of the initial particle size of the CPC, had huge relevance in the field of protein adsorption and the ability for proteins to penetrate inside the matrix. It was seen that as the L/P ratio was increased, the amount of protein that was able to penetrate was increased, but this penetration was also depended on the initial particle size. Since the different particle 108 108108 108 Calcium Phosphate Cement-Collagen for Bone Regeneration sizes created two well defined microstructures, the lower the specific surface area, the higher the porosity, and therefore, a higher protein penetration. 2.5.7. Injectability When performing an in vivo or a clinical application, one of the first parameter that surgeons will deal with is the injectability. One of the main complains surgeons have, is that CPC are poorly injectable 88-91 . Some CPC are not injectable due to the high force that must be applied for the injection or that because not all the paste can be extruded. Our results revealed that the presence of collagen increased the injectability of the CPC, from 50% to 96% for the CTRLF and COLF10 samples respectively (Figure 2.29). Nevertheless, the presence of fibrillised collagen did not show the same efficiency for the CPC extrusion. The increase in injection was only up to 65%. Furthermore, the presence of fibrillised collagen showed an increase in the force needed to start injection respect to the CPC with solubilized collagen and the CTRLF (Figure 2.30). This can be adscribed to the presence of an initial paste composed of CPC and collagen bundles. Solubilized collagen did enhance the injectability, but the presence of the bundles decreased the ability to be injected. Furthermore, both CPC with collagen in the liquid phase presented a slight increase in the force needed to start injecting the paste (Figure 2.31). This can be attributed to the higher viscosity of the paste. It is known that the ability of a CPC to be injected can be enhanced by the increase in the L/P ratio, the use of round particles, the addition of citrate ions and the use of viscous polymer solutions 91 . The presence of polymers combined with the CPC have been shown to enhance the injectability 92-95 . The main reason for the enhanced injectability is the lubricating effect that the polymer has on the different cement particles 91,96,97 . The presence of a polymer between the different grains may reduce the friction between the different grains and therefore increase the injectability 96,97 . This was thought as the main reason for an increased injectability observed in the CPC combined with collagen. One of the most important problems in the ability to inject a CPC is the phase separation or the filter-pressing effect. When a CPC is injected, a certain pressure is applied to the syringe and this pressure is directly applied to the cement paste. Since the Chapter 2 109 109109 109 paste has to pass through a small cannula at the end, there can be the filter pressing 91 . This occurs when a phase separation takes places, meaning that when the injection is produced, the liquid is extruded, whereas most of the powder remains in the syringe 91,98,99 . That means that the L/P ratio inside the syringe can be controlled, but once it is injected, the L/P ratio of the extruded paste can be different from the initial one. If the paste is able to be injected completely, the phase separation is less likely to happen. In the case in which not all the paste is injected, the force will start to increase, and therefore, the phase separation will take place. The incorporation of collagen or other polymers in general, may reduce the phase separation effect, and therefore the injectability may be increased 91 . Although the incorporation of collagen was not designed to increase this feature, the results showed that it did enhance the injectability. 2.5.8. Mechanical properties The results for the compressive strength showed that for the low concentration (10 mg/ml) collagen containing CPC, the compressive strength was similar to that of the control (Figure 2.32). Nevertheless, a clear decrease of the mechanical properties was found when the collagen concentration was increased, both for fine and coarse CPC. The decreased values for the CPC containing the higher concentrations of collagen cannot be attributed to an increase in the total porosity of the samples, since it was previously shown to be similar (Table 2.6). The results are in agreement with previous works that reported that for similar collagen concentrations incorporated in the CPC, the effect on the compressive strength was non-existing 22 , although when the collagen concentration was increased, the compressive strength was reduced 23 . The presence of fibrillised collagen slightly decreased the mechanical properties compared to the solubilized collagen containing samples. Nevertheless, it is worth highlighting that the presence of the fibrillised collagen, especially for the COLF50F, there was an increase in the strain, although it presented a lower compressive strength, leading noncatastrophic failures compared to the brittle failure of the CTRLF (Figure 2.33). This was also previously seen when a CPC was combined with collagen fibers 24 . The enhanced mechanical properties in that case were attributed to the presence of HA on the collagen fibres which were able to resist crack propagation. 110 110110 110 Calcium Phosphate Cement-Collagen for Bone Regeneration Lower values of compressive strength were found for the coarse than for the fine CPC. This cannot be attributed to the porosities since they present similar total porosities (Table 2.6.). However, it was previously reported that for the same inorganic CPC, the mechanical properties for coarse and fine were not statistically different 9 . 2.6. Conclusions The results have shown that collagen containing CPC can be obtained by dissolving collagen in the liquid phase of a CPC. Different collagen treatments were applied in order to observe the effect of collagen morphology on the properties of the CPC. Collagen was shown to be a retarder of the hydrolysis of the α-TCP into CDHA at the initial reaction times. The main principle underlying this delay was the presence of the acetic acid and the higher viscosity of the collagen solution. Nevertheless, already after 1 hour, there were no differences in the kinetics of the transformation into CDHA in the presence of collagen and that the final product was not altered. An important finding was that the collagen was not released during the 7 day setting reaction in water. This was further confirmed by the observation of collagen with a fluorescent marker in the set CPC. The distribution was shown to be homogenous for the solubilized collagen and heterogeneous for the fibrillised collagen. It was also seen that the presence of collagen, increased the injectability and that it did not influence the mechanical properties at low collagen concentrations, whereas at higher collagen concentrations there was a decrease in the mechanical properties. Chapter 2 111 111111 111 2.7. References 1. Du C, Cui FZ, Zhu XD & de Groot K. Three-dimensional nano-HAp/collagen matrix loading with osteogenic cells in organ culture. Journal of Biomedical Materials Research 44, 407-415 (1999). 2. Lickorish D, Ramshaw JAM, Werkmeister JA, Glattauer V & Howlett CR. Collagen-hydroxyapatite composite prepared by biomimetic process. Journal of Biomedical Materials Research 68A, 19-27 (2004). 3. Zou C et al. Preparation and characterization of porous [beta]-tricalcium phosphate/collagen composites with an integrated structure. Biomaterials 26, 5276-5284 (2005). 4. Kikuchi M, Itoh S, Ichinose S, Shinomiya K & Tanaka J. Self-organization mechanism in a bone-like hydroxyapatite/collagen nanocomposite synthesized in vitro and its biological reaction in vivo. Biomaterials 22, 1705-1711 (2001). 5. Myun CC, Ikoma T, Kikuchi M & Tanaka T. Preparation of a porous hydroxyapatite/collagen nanocomposite using glutaraldehyde as a crosslinkage agent. Journal of Materials Science Letters 20, 1199-1201 (2001). 6. Kikuchi M et al. Biomimetic synthesis of bone-like nanocomposites using the self-organization mechanism of hydroxyapatite and collagen. Composites Science and Technology 64, 819-825 (2004). 7. Ginebra MP et al. Setting reaction and hardening of an apatitic calcium phosphate cement. Journal of Dental Research 76, 905-912 (1997). 8. Ginebra MP, Fernandez E, Driessens FCM, Boltong MG & Planell JA. Influence of the particle size of the powder phase in the setting and hardening behaviour of a calcium phosphate cement. Bioceramics 10, 481 (1997). 9. Ginebra MP, Driessens FCM & Planell JA. Effect of the particle size on the micro and nanostructural features of a calcium phosphate cement: a kinetic analysis. Biomaterials 25, 3453-3462 (2004). 112 112112 112 Calcium Phosphate Cement-Collagen for Bone Regeneration 10. Angele P et al. Influence of different collagen species on physico-chemical properties of crosslinked collagen matrices. Biomaterials 25, 2831-2841 (2004). 11. Quereshi S et al. Extraction and partial characterization of collagen from different animal skins. Recent Research in Science and Technology 2, 28-31 (2010). 12. Seteven FS & Thomas H. Preparation of insoluble collagen from human cartilage. Biochemical Journal 135, 245-247 (1973). 13. Bensusan HB & Hoyt BL. The effect of various parameters on the rate of formation of fibers from collagen solutions. Journal of the American Chemical Society 80, 719-724 (1958). 14. Wood GC & Keech MK. The formation of fibrils from collagen solutions. 1. The effect of experimental conditions: kinetic and electron-microscope studies. Biochemical Journal 75, 588 (1960). 15. Cassel JM. The kinetics of the heat precipitation of collagen. Journal of American Leather Chemists Association 51, 556-557 (1962). 16. Hayashi T & Nagai Y. Effect of pH on the stability of collagen molecule in solution. Journal of Biochemistry 73, 999-1006 (1972). 17. Piez KA. Structure and assembly of the native collagen fibril. Connective Tissue research 10, 25-36 (1982). 18. Veis A. Collagen fibrillogenesis. Connective Tissue Rresearch 10, 11-24 (1982). 19. Kadler KE, Holmes DF, Trotter JA & Chapman JA. Collagen fibril formation. Review article. Biochemistry Journal 316, 1-11 (1996). 20. Delorenzi NJ, Sculsky G & Gatti CA. Effect of monovalent anions on type I collagen fibrillogenesis in vitro. International Journal of Biological Macromolecules 19, 15-20 (1996). 21. Goh MC et al. Fibril formation in collagen. Physica A 239, 95-102 (1997). Chapter 2 119 119119 119 82. Slosarcyk A, Szymure-Oleksiak J & Mycek M. The kinetics of pentoxifylline release from drug loaded hydroxyapatite implants. Biomaterials 21, 1215-1221 (2000). 83. Bohner M et al. Gentamicin-loaded hydraulic calcium phosphate bone cement as antibiotic delivery system. Journal of Pharmaceutical Sciences 86, 565-572 (1997). 84. Nihouannen DL, Hacking SA, Gbureck U, Komarova SV & Barralet JE. The use of RANKL-coated brushite cement to stimulate bone remodeling. Biomaterials 29, 3253-3259 (2008). 85. Mathiowitz E. Encyclopedia of controlled drug delivery. John Wiley and Sons, New York (1999). 86. Ratner BD, Hoffman AS, Schoen FJ & Lemons JE. Biomaterials Science. An introduction to Materials in Medicine. Academic Press, San Diego (2004). 87. Espanol M et al. Intrinsic porosity of calcium phosphate cements and its significance for drug delivery and tissue engineering applications. Acta Biomaterialia 5, 2752-2762 (2009). 88. Ishikawa K. Effects of spherical tetracalcium phosphate on injectability and basic properties of apatitic cement. Key Engineering Materials 204-242, 369- 372 (2003). 89. Bohner M & Baroud G. Injectability of calcium phosphate pastes. Biomaterials 26, 1553-1563 (2005). 90. Leroux L, Hatim Z, Freche M & Lacout JL. Effects of various adjuvants (lactic acid, glycerol and chitosan) in the injectability of a calcium phosphate cement. Bone 25, S31-S34 (1999). 91. Khairoun I, Boltong MG, Driessens FCM & Planell JA. Some factors controlling the injectability of calcium phosphate bone cements. Journal of Materials Science: Materials in Medicine 9, 425-428 (1998). 120 120120 120 Calcium Phosphate Cement-Collagen for Bone Regeneration 92. Andrianjatovo H & Lemaitre J. Effects of polysaccharides on the cement properties in the monocalcium phosphate/β-tricalcium phosphate systems. Innovation in Technology, Biology and Medicine 16S, 140-147 (1995). 93. Belkoff SM, Mathis JM, Jasper LE & Deramond H. An ex vivo biomechanical evaluation of a hydroxyapatite cement for use with vertebroplasty. Spine 26, 1542-1546 (2001). 94. Borzacchiello A, Sanginario V, Ambrosio L, Ginebra MP & Planell JA. Characterization of an injectable hydrogel composite for orthopedic applications. Proceedings of the Second International Conference on New Biomedical Materials. 2003. Cardiff, UK. 4-6-2003. 95. Ginebra MP et al. Mechanical and rheological improvement of a calcium phosphate cement by the addition of a polymeric drug. Journal of Biomedical Materials Research 57, 113-118 (2001). 96. Lombois H, Halary JL, Van Damme H & Colombet P. Adsorption, lubrification et interaction de contact dans les pâtes denses polymère-ciment. Proceedings of the 38ème colloque annuel du groupe français de rhéologie . 2003. Brest, France. 97. Mansoutre S, Colombet P & Van Damme H. Water retention and granular rheological behavior of fresh C 3S paste as a function of concentration. Cement concrete research 29, 1441-1453 (1999). 98. Khairoun I, Driessens FCM, Boltong MG, Planell JA & Wenz R. Addition of cohesion promoters to calcium phosphate cements. Biomaterials 20, 393-398 (1999). 99. Habib M, Baroud G, Gitzhofer F & Bohner M. Mechanisms underlying the limited injectability of hydraulic calcium phosphate paste. Acta Biomaterialia 4, 1471 (2008) Chapter 3 121 Chapter 3: Cell Response to Injectable CPC/Collagen Composites 3.1. Introduction The previous chapter focused on the preparation and characterization of the collagen CPC composites. The final goal of these materials is to be able to enhance the biological performance. Hydroxyapatite and collagen have been combined, mainly as macroporous tissue engineering scaffolds. Hydroxyapatite is known to be a biocompatible biomaterial in vitro as well as in vivo, with an osteconductive potential1-3. Therefore it has been combined with collagen by several methods as described in chapter 1. However, in the collagen scaffolds, the matrix is composed of collagen, onto which small amounts of HA precipitate4-7. In the present chapter, the matrix of the material is the calcium 122 Cell Response to Injectable CPC/Collagen Composites phosphate, and the effect of collagen on the in vitro biological performance is studied in this chapter. In previous works in which collagen was mixed with a CPC, the biological aspects were not deeply studied8-11. The main effect that was reported in the previous works was the ability of the collagen to increase the initial adhesion on the CPC material. The effect of collagen on cell proliferation and differentiation on CPC based materials has not been previously studied. The concentration of the collagen solution incorporated in the CPC was 10 mg/ml, since higher collagen concentrations have reported no difference at early cell attachment on other CPC11. 3.2. Objectives The objective of this chapter was to study the in vitro cell response to injectable calcium phosphate cement –collagen composite material. The effect of collagen addition, as well as the pre-treatment of the collagen to form solubilized or fibrillised collagen was investigated. The study was aimed at analyzing the initial adhesion of osteoblastic cells SaOs-2 on the material, as well as to observe the proliferation and differentiation after 1, 7 and 14 days. 3.3. Materials and methods 3.3.1. Materials The study was done on 15 mm diameter disks. The disks were prepared by moulding the CPC paste in Teflon moulds of 15 mm in diameter and 2 mm in height. After 3 hours, the disks were unmolded and left reacting in Ringer´s for 7 days in order to ensure the transformation of the α-TCP into CDHA. The L/P used was 0.45 ml/g. The liquid phase of the CPC was a 50 mM acetic acid solution for the control and two different 10 mg/ml collagen solutions: solubilized and fibrillised. The materials were coded using 4 letters. The first three letters corresponded to COL, which identified the samples as containing collagen, followed by C, meaning the initial particle size of the CPC, which was coarse in this case, followed by a number referring to the concentration of the collagen solution. Finally, the presence of and F at the end Chapter 3 123 indicated that the collagen had been fibrillised. The materials studied were then: COLC10, COLC10F and CTRLC. The CTRLC was CPC composed of coarse cement with acetic acid solution was coded as. The tissue culture plastic (empty well) was also used as control, being coded as TCPS. The materials were sterilized by immersion for 1 hour in 70% ethanol. 3.3.2. Cells Human osteoblast-like Saos-2 cells were used as cell model. The cells were maintained in McCoy medium (Sigma, M8403) supplemented with 0.75% of L-glutamine (GIBCO 25030), 1% penicillin/streptomycin (GIBCO 15140), 2 % of sodium pyruvate (GIBCO 11360) and 15 % of fetal bovine serum (GIBCO 10270-106) in a humidified atmosphere of 5% CO2 in air. The culture medium was exchanged every second day. Upon confluence the cells were detached with a minimum amount of trypsin-EDTA (Gibco) that was inactivated with FBS after 5 minutes. The cells were then re-cultured or used for experiments. Saos-2 cells were harvested from nearly confluent flasks as described above and seeded in 24 well plates. Afterwards, 1.5 ml of complete medium was added, changed after 24 hours and then changed every 48 hours. 3.3.3. Cell behavior on CPC/collagen composites 3.3.3.1 Initial adhesion In order to verify the effect of the presence of collagen in the CPC in terms of initial cell attachment, an initial adhesion assay was performed. 15 mm diameter disks were prepared as previously described. COLC10, COLC10F, CTRLC and TCPS samples were studied. The materials were left overnight in contact with serum free medium to wet the samples. On the next day, the cells were seeded on the materials at a concentration of 1.000.000 cells/well and were left in contact with the material for 4 hours. The samples were then removed and placed in another well plate and the number of cells attached to the material was quantified. The viability of the cells was estimated spectrophotometrically with the LDH assay and the cell morphology was assessed by fluorescence microscopy after FDA staining. 124 Cell Response to Injectable CPC/Collagen Composites 3.3.3.2 Cell proliferation and cell differentiation For the same materials used in the initial adhesion test, 100.000 cells were seeded per well, which represented approximately 14.000 cell/cm2. Proliferation, performed with an LDH kit, differentiation, measured by the quantification of ALP activity, as well as FDA and SEM images after 1, 7 and 14 days were taken. 3.3.4. Characterization 3.3.4.1. Proliferation Relative cell numbers were evaluated at 1, 7, and 14 days by the lactate dehydrogenase (LDH) assay. The LDH activity was then determined spectrophotometrically with a commercially available LDH kit (Roche, Germany) in a plate reader (Power WaveX, Bio-Tek Instruments, USA; 490 nm). For that purpose, at each time point, the samples were washed twice with PBS and lysed by freeze-thawing, following at least two repeating cycles in the culture plate. The lysates were then transferred into eppendorfs. The lysates were centrifuged at 1500 rpm for 10 min to remove cell debris. Aliquots of the samples were placed on 96 well plates to obtain a final sample volume of 100 µl, after the corresponding dilution. Afterwards, 100 µl of the reaction mixture was placed on the wells, with the previously added sample. The reaction mixture was composed of the mixture of the catalyst, which is a mixture of Diaphorase/NAD+, and the dye solution, which is composed of Iodotetrazolium chloride and sodium lactate (Figure 3.1). The mixture of the reaction mixture and the samples aliquots, were left reacting for 30 minutes, after which 50 µl of a stop solution, composed of 1M HCl, was placed in each well in order to stop the reaction. A calibration curve with decreasing concentrations of cells was created to express results in cell number. Chapter 3 125 Figure 3.1. Diagram of LDH oxidation of lactate into pyruvate through the reduction of NAD+ to NADH. The reaction in step 2 shows how the tetrazolium salt is reduced to a formazan salt which has the red coloration of the end product which is done through the help of the catalyst and the oxidation of the NADH to NAD+ (From LDH kit Roche). 3.3.4.2. Differentiation The retention of osteoblastic phenotype was evaluated by measuring alkaline phosphatase activity. No osteogenic medium was used. A colorimetric method, based on the conversion of p-nitrophenyl phosphate into p-nitrophenol in the presence of alkaline phosphatase, was used. The lysates obtained in the previous section were mixed with 2-Amino-2-methyl-1-propanol buffer (Sigma Diagnostics Inc A9226.) and phosphatase substrate solution (Sigma, 4 mg/ml P5994), and incubated for 30 minutes at 37ºC. The reaction was stopped with 0.05 M NaOH and the production of pnitrophenol was determined by measuring the absorbance at 405 nm. The values were calibrated to a standard curve, prepared from known concentrations of p-nitrophenol (Sigma N7660), and the results for alkaline phosphatase activity were normalized to the number of cells on each sample. 3.3.4.3. Fluorescein Diacetate staining To follow the overall morphology of adhering living cells, fluorescence images were obtained after the fluorescein diacetate staining (FDA, Invitrogen F1303) (Figure 3.2.), to obtain control on cell viability. At given time of incubation, the living cells were labeled with fluorescein diacetate (FDA), by adding 10 µl/ml from a stock of 1 mg/ml 126 Cell Response to Injectable CPC/Collagen Composites FDA in acetone to the medium. Under these conditions, the vital cells converted FDA in a fluorescent analogue via their esterases. The dye was then removed and rinsed three times with water and observed with PBS at 37ºC. Representative pictures of the adhered cells were then taken with a fluorescent microscope (Nikon, Eclipse E600) using the green channel. Figure 3.2. Representation of the Fluorescein Diacetate molecule. 3.3.4.4. Scanning Electron Microscopy Cell morphology was further characterized by means of SEM. For that purpose, the samples were washed in 0.1M Phosphate buffer, pH 7.4, and cells were fixed with a 2.5% glutaraldehyde (Sigma-Aldrich G400-4) solution in PBS, washed and maintained in 0.1M phosphate buffer. Osmium tetraoxide (Sigma-Aldrich 201013) was added after fixation, and graded ethanol solutions were used to dehydrate the samples (50, 70, 90, 96 and 100% ethanol). Finally hexamethyldisilazane (HDMS, Fluka 52620) was used for complete dehydratation of the samples, being air-dried afterwards. 3.3.5. Statistical analysis Statistical analysis was carried out with significance of 5%. One way analysis of variance (ANOVA) with Fisher post-hoc test was conducted. The data are expressed as mean ± standard deviation. 3.4. Results 3.4.1. Initial cell adhesion The fluorescent images after FDA staining for the different materials showed the initial attachment after 4 hours in serum-free medium (Figure 3.3). In general, cells appeared Chapter 3 127 to be rounded, although some cells were starting to expand. There were some differences between the different materials concerning the amount of the cells observed. In CTRLC (Figure 3.3.a and b) and COLC10F (Figure 3.3.e and f) , the number of cells present was similar. However, for the COLC10 (Figure 3.3.c and d), there were a higher number of cells compared to the other two substrates. Figure 3.3. Initial adhesion of Saos-2 cells after 4 hours on the different materials at two different magnifications. a) and b) CTRLC, c) and d) COLC10, e) and f) COLC10F. Scale bar = 100 µ m. Figure 3.4 shows the number of cells that attached to different CPC materials and the TCPS measured by LDH. TCPS presented the highest value of cells attached, although only 300.000 cells out of the 1.000.000 initially seeded attached, which represented a c a b f d e 128 Cell Response to Injectable CPC/Collagen Composites 30% of cell attachment. On the other hand, the amount of cells that attached to the CTRLC was 100.000, representing a 10% of the cells initially attached. These values were further increased in the presence of collagen for the samples COLC10 and COLC10F, arriving to values close to those of TCPS, being 25% and 15% respectively of cell attachment. Figure 3.4. Quantification of number of cells after 4 hours, representing the number of cells that have attached to the well and the number of cells extracted from the material. 3.4.2. Cell proliferation and cell differentiation 3.4.2.1. Proliferation The results for proliferation at 1, 7 and 14 days are shown in Figure 3.5. Initially, after 1 day the number of cells was low in the 4 cases, having a higher number in the TCPS. After 7 days, the number of cells on TCPS raised considerably, whereas it remained low for CTRLC and COLC10F. However, in COLC10 the number of cells was three times higher than for the CTRLC and COLC10F. Finally, after 14 days, the proliferation for COLC10 was higher than the CTRLC, and was also higher than the COLC10F. The CTRLC and the COLC10F samples seemed to behave in a similar way, not presenting significant differences among them. 0,0E+00 5,0E+04 1,0E+05 1,5E+05 2,0E+05 2,5E+05 3,0E+05 3,5E+05 4,0E+05 Cell number TCPS CTRLC COLC10 COLC10F 4 hours Chapter 7 233 were significant in all cases, whereas there were only significant differences between CYTODEX and GEL/HA-MC at the 6 hour period. Figure 7.9. Proliferation for 6, 24 and 72 hours measured with LDH for HA-MC, GEL/HA-MC and CYTODEX in a) static culture and b) dynamic culture. * denotes significant differences (p<0.05). 7.4.1.1. Long-term dynamic culture The fluorescence images after FDA staining images of the different MC after 1, 7 and 14 days of culture are shown in Figure 7.10. At low culture times, the MC were able to move easily around the spinner flask and were resuspend when the spinner flask was a) b) 234 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers stirred. However, at 7 days, as evidenced by the FDA images, the MC tended to agglomerate (Figure 7.10). This was visually observed by sedimentation of big clusters of MC at the bottom of the flask. Since the MC were at the bottom of the flask, cells tended to start proliferating in the interface between the different MC and tended to aggregate them, therefore the resuspension upon stirring was hindered. Figure 7.10. Fluorescence images after FDA staining images obtained at 1, 7 and 14 days for the HA-MC and GEL/HA-MC. Bar = 200 µ m. Chapter 7 235 After 14 days of culture, the distribution of cells on the MC was rather heterogeneous. Whereas some MC had plenty of cells on top of them, other had few or no cells (Figure 7.11). Figure 7.11. SEM image after 14 days of dynamic culture for the HA-MC. a) Low magnification of the different MC presenting some MC with cells and some MC with no cells. b) Higher magnifications of MC covered with several layers of cells on top of the MC. The results of cell proliferation measured by LDH in static culture are shown in Figure 7.12a. Low number of cells were found for the HA-MC at 1 and 7 days of culture. The number of cells in the HA-MC considerably increased after 14 days compared to 1 and 7 days. A higher cell number at 1 and 7 days in the GEL/HA-MC compared to HA-MC was observed. There were no significant differences in the number of cells between HAMC and GEL/HA-MC after 14 days. In the dynamic culture, the trend was different to the static as shown in Figure 7.12b. At 1 day, there were statistically significant differences between HA-MC and GEL/HAMC. After 7 days, the amount of cells was higher in the case of HA-MC than on the gelatin containing MC, whereas after 14 days, the trend was the opposite and the amount of cells was higher for the gelatin containing MC, being the differences significant in both cases. a b 236 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers Figure 7.12. Proliferation for 1, 7 and 14 days measured with LDH for HA-MC and GEL/HA-MC in a) static culture and b) dynamic culture. * denotes significant differences (p<0.05). 7.4.2. MC-containing alginate gels The MC were then combined with sodium alginate gel to assess their ability to be injected. All the MC were injectable when mixed with a 2% sodium alginate solution. The sodium alginate gel was also able to adapt to the mould in which it was injected. Once the gel was extracted and lyophilized, the MC were shown to form well defined cylinders, demonstrating that the gel had been able to adapt to the walls of the moulds. The samples were lyophilized and observed by stereoscope as shown in Figure 7.13. The cross-section of the samples presented a structure composed of MC aggregation. 0 10 20 30 40 50 1 7 14 Number of cells/mg x 103 Time (Days) MC-HA MCG-HA 0 20 40 60 80 100 120 140 160 1 7 14 Number of cells/mg x 103 Time (Days) MC-HA MCG-HA GEL/HA-MC HA-MC * * HA-MC GEL/HA-MC * * a) b) Chapter 7 237 The outside of the lyophilized MC containing gel showed that the different MC were placed together and linked through the alginate gels. At higher magnifications, it was observed that the different MC were not in contact with surrounding MC, but were separated by the alginate gel. Figure 7.13. Optical images of the constructs obtained with the alginate and GEL/HA-MCs showing a) the top surfaces, b) the lateral surface and c) top surface at higher magnifications. SEM images of the lyophilized gels are shown in Figure 7.14. The morphology was similar for the HA-MC and the GEL/HA-MCs, but different to the GEL/HA-MCb (Figure 7.14). The gaps between MC in the latter case were bigger. a) b) c) 238 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers MA-MC GEL/HA-MCs GEL/HA-MCb Figure 7.14. SEM images for the different constructs obtained from the mixing with alginate. a) and b) HA-MC construct, c) and d) GEL/HA-MCs construct, e) and f) GEL/HA-MCb construct. The total porosity of the samples and the pore size distribution were measured by MIP. The results are shown in Figure 7.15. It can be seen that, as expected, the bigger the MC size, the bigger the gaps between them, and therefore, the bigger the pore size observed (Figure 7.15a). In the case of the HA-MC and the GEL/HA-MCs, the pore size was in the range between 6 and 100 µm, having its peak in the range of 30 to 40 µm. However, in the GEL/HA-MCb, the pore size distribution ranged between 10 µm and 160 µm, 4 mm 4 mm 4 mm a 1 mm 1 mm 1 mm b c d e f Chapter 7 239 having its peak at a value of 65 µm. Furthermore, the same graphic is shown in logarithmic scale (Figure 7.15b), showing at low pore size the pores corresponding to the intrinsic porosities of the MC, as was already shown in Chapter 5. Figure 7.15. Pore size distribution for the HA-MC, GEL/HA-MCs and GEL/HA-MCb construct. a) Lineal scale and b) logarithmic scale. Although presenting considerably different pore size distributions, the total porosity of the samples was similar in all cases (Table 7.1). Sample % Porosity HA-MC 73.9 GEL/HA-MCs 74.2 GEL/HA-MCb 74.1 0 0,2 0,4 0,6 0,8 1 1,2 1,4 0100 200 300 400 dV/dlogD Pore diameter ( µ m) HA-MC GEL/HA-MCs GEL/HA-MCb 0 0,2 0,4 0,6 0,8 1 1,2 1,4 0,001 0,1 10 1000 dV/dlogD Pore diameter ( µ m) HA-MC GEL/HA-MCs GEL/HA-MCb Table 7.1 Porosity of the different constructs obtained with the microcarriers. a b 240 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers 7.5. Discussion The dynamic cultures are of importance in several fields and have been widely used to expand cells on MC instead of the typical culture flasks25-28. There are two main applications for the use of MC as shown in Figure 7.16. MC can be designed so that cells are able to attach on them in order to obtain high number of viable cells for further experiments, or they can be designed so that cells attach on them for further implantation of the MC loaded with the cells into the defect site. This is the approach proposed in this Thesis. Figure 7.16. Representation of the use of MC. Cells are cultured on 2D cell culture on T-flasks. These anchorage dependent cells may attach to microcarriers in a dynamic culture. The microcarriers can be used, depending on the material and the purpose, as a way to obtain a high amount of viable cells due to the high surface available for cells to attach, or can be directly implanted into a defect to deliver a biomaterial with and elevated amount of cells. An important issue is that depending on the MC nature, the gentle agitation can be insufficient to resuspend the MC. Polymeric MC, present low densities and are resuspended easily5,6. However, ceramics present higher densities, which may provoke sedimentation of the MC at the bottom of the flask. Actually, this is considered as one of the main drawbacks when using calcium phosphate MC in dynamic cultures, since their density is higher compared to the culture medium. In order to decrease the density of the MC, attempts have been made to fabricate hollow HA MC29,30. In order to enhance MC resuspension, the effect of using a high rotation speed (80 rpm) was analyzed. As shown in Figure 7.3, the results showed a higher number of cells in the different MC seeded at 40 rpm compared to the cells seeded on the MC at 80 rpm. 2D cell culture MC Dynamic culture Trypsinize cells adhered on MC for its subsequent use Implant MC with adhered cells in the defect Chapter 7 241 Furthermore, the number of MC with cells on top was higher in the 40 rpm seeded MC. Moreover, MC were shown to fracture after the 24 hour initial experiment for the 80 rpm speed. It was concluded that, although the higher speeds gave rise to a higher resuspension of the MC in the medium, the higher speed was detrimental for cell viability and MC integrity. Therefore, the 40 rpm speed was selected for the dynamic cultures. It has been documented that speed influences adhesion and proliferation on MC3,4. It was observed that speeds around 40 and 60 rpm gave the highest values of proliferation for Vero cells on Cytodex MC, whereas lower or higher speeds decreased the number of proliferating cells3,4. This can be related to the fact that cells can be damaged by strong collisions during agitation at high rotating speeds31. Therefore, equilibrium has to be found between rotating speed, cell viability and MC integrity. The 40 rpm speed did not resuspend the HA MC as much as in the case of the polymer. That is, in the case of CYTODEX, the MC were dispersed in all the volume, or in other words, they were resuspended to the highest height of the flask as seen in Figure 7.17. For the HA-containing MC, the MC only reached a small height as observed in Figure 7.17. The black arrows represent the height the MC were able to reach in each case, whereas the red arrows represent the height cells reached. In both cases, the red arrows are the same length, indicating that the height reached for the cells is the same in both cases. Figure 7.17. Representation of the suspension ability of the different MC (Cytodex and CPC-MC) upon stirring. The black arrows represent the total height the MC are resuspended, whereas the red arrows represent the height into which the cells are resuspended. CYTODEX CPC-MC Cells 242 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers Nevertheless, the conclusion that was extracted from the results was that it was more favorable for cell viability to have a lower rotation speed that would not damage the cells, instead of having higher rotating speeds that would not allow for cells to adhere and survive on the MC. One of the goals of this chapter was to apply the spinner flask dynamic culture system to the HA containing MC and compare it with the static culture system. However, the two systems are very different, and therefore, direct comparison is difficult. Table 7.2 summarizes the main values for the parameters in each of the two culturing conditions. The values for the dynamic culture were selected according to the CYTODEX manufacturer and to previous studies3,4,23. The fact of having a big volume of medium in the spinner flask allowed for a higher number of cells to be introduced. However, the number of cells that can be seeded in the well plate in static was limited because of the medium volume and of the available space. Static Dynamic MC Weight (mg) 39 300 MC Surface (cm2) 11.8 82.5 Cells seeded 2x105 107 Medium (ml) 1 100 Cells/surface of MC (cells/cm2) 16,949 121,212 Cells/weight of MC (cells/mg) 5,128 33,333 Table 7.2. Comparison between the different parameters of cell culture in static and dynamic culture. Moreover, it was interesting to carry out two different types of experiments: short-term and long-term. For the short-term culture, the differences between the dynamic and the static cultures were quite significant. In order to compare the dynamic and static culture easier, the values for the different MC were combined in Figure 7.18. In the HA-MC and GEL/HA-MC in static cultures, the proliferation was very low. In the 3 day period, no increase in cell number was observed. This is related with the intrinsic properties of the material and with the low seeding efficiency of the MC. Cells seeded on HA and similar materials have in general low attachment ratios due in some cases to the surface roughness32,33. Therefore, proliferation is usually delayed and the amount of cells on the material is low at short times. Regarding the seeding efficiency, in static it is usually low26 since cells may fall in the gaps between the MC. This is because once the cells are Chapter 7 249 extensive articular cartilage defects. Osteoarthritis and Cartilage 3, 61-70 (1995). 11. Taguchi T et al. Encapsulation of chondrocytes in injectable alkali-treated collagen gels prepared using poly(ethilene glycol)-based 4-armed star polymer. Biomaterials 26, 1247-1252 (2005). 12. Chenite A et al. Novel injectable neutral solutions of chitosan from biodegradable gels in situ. Biomaterials 21, 2155-2161 (2000). 13. Chung HJ et al. Synthesis and characterization of Pluronic grafted chitosan copolymer as a novel injectable biomaterial. Current Applied Physics 5, 485-488 (2005). 14. Paige KT, Cima LG, Yaremchuk MJ, Vacanti JP & Vacanti CA. Injectable cartilage. Plastic Reconstruction Surgery 96, 1390-1400 (1995). 15. Stevens MM, Qanadilo HF, Langer R & Shastri VP. A rapid-curing alginate gel system: utility in periosteum-derived cartilage tissue engineering. Biomaterials 25, 887-894 (2004). 16. Balakrishnan B & Jayakrishnan A. Self-cross-linking biopolymers as injectable in situ forming biodegradable scaffolds. Biomaterials 26, 3941-3951 (2005). 17. Park YD, Tirelli N & Hubbell JA. Photopolymerized hyaluronic acid-based hydrogels and interpenetrating networks. Biomaterials 24, 893-900 (2003). 18. Shu XZ, Liu YC, Palumbo FS, Luo Y & Prestwich GD. In situ crosslinkable hyaluronan hydrogels for tissue engineering. Biomaterials 25, 1339-1348 (2004). 19. Wang C, Gong Y, Lin Y, Shen J & Wang DA. A novel gellan gel-based microcarrier for anchorage-dependent cell delivery. Acta Biomaterialia 4, 1226- 1234 (2008). 20. Hong Y, Gong Y, Gao C & Shen J. Collagen-coated polylactide microcarriers/chitosan hydrogel composite: injectable scaffold for cartilage regeneration. Journal of Biomedical Materials Research 85A, 628-637 (2008). 250 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers 21. Smetana K Jr. Cell biology of hydrogels. Biomaterials 14, 1046-1050 (1993). 22. Rowley JA, Malambayan G & Mooney DJ. Alginate hydrogels as synthetic extracellular matrix materials. Biomaterials 20, 45-53 (1999). 23. Yang Y, Rossi FMV & Putnins EE. Ex vivo expansion of rat bone marrow mesenchymal stromal cells on microcarriers beads in spin culture. Biomaterials 28, 3110-3120 (2007). 24. Malda J, Kreijveld E, Temenoff JS, van Blitterswijk CA & Riesle J. Expansion of human nasal chondrocytes on macroporous microcarriers enhances redifferentiation. Biomaterials 24, 5153-5161 (2003). 25. Melero-Martin JM, Dowling MA, Smith M & Al-Rubeai M. Expansion of chondroprogenitor cells on macroporous microcarriers as an alternative to conventional monolayer systems. Biomaterials 27, 2970-2979 (2006). 26. Schop D et al. Expansion of human mesenchymal stromal cells on microcarriers: growth and metabolism. Journal of Tissue Engineering and Regenerative Medicine 4, 131-140 (2010). 27. Frondoza C, Sohrabi A & Hungerford D. Human chondrocytes proliferate and produce matrix components in microcarrier suspension culture. Biomaterials 17, 879-888 (1996). 28. Malda J et al. Expansion of bovine chondrocytes on microcarriers enhances redifferentiation. Tissue Engineering 9, 939-948 (2003). 29. Doctor J et al. Evaluating mcirocarriers for delivering human adult mesenchymal stem cells in bone tissue engineering. Developmental Biology 247, 505 (2002). 30. Qiu Q, Ducheyne P & Ayyaswamy P. 3D bone tissue engineered with bioactive microspheres in simulated microgravity. In vitro Cellular Developmental Biology Animals 37, 157-165 (2001). Chapter 7 251 31. Lakhotia S & Paputsakis ET. Agitation induced cell injury in microcarrier cultures, protective effect of viscosity is agitation intensity dependent: experiments and modeling. Biotechnology and Bioengineering 39, 95 (1992). 32. Zhang W, Walboomers XF, Van Osch G, Van den Dolder J & Jansen JA. Hard tissue formation in a porous HA/TCP ceramic scaffold loaded with stromal cells derived from dental pulp and bone marrow. Tissue Engineering 14, 285-294 (2008). 33. Bjerre L, Bünger C, Baatrup A, Kassem M & Mygind T. Flow perfusion culture of human mesenchymal stem cells on coralline hydroxyapatite scaffolds with various pore sizes. Journal of Biomedical Materials Research 97A, 251-263 (2011). 34. Altman G et al. Cell differentiation by mechanical stress. FASEB 16, 270-272 (2002). 35. Shikani AH et al. Propagation of human nasal chondrocytes in microcarrier spinner culture. American Journal of Rhinology 18, 105-112 (2004). 36. Malda J et al. Effect of oxygen tension on adult articular chondrocytes in microcarrier bioreactor culture. Tissue Engineering 10, 987-994 (2004). 37. Tan H, Wu J, Huang D & Gao C. The design of biodegradable microcarriers for induced cell aggregation. Macromolecular Bioscience 10, 156-163 (2010). 38. Borden M, Attawia M, Khan Y & Laurencin CT. Tissue engineered microsphere-based matrices for bone repair: design and evaluation. Biomaterials 23, 551-559 (2002). 39. Borden M, El-Amin SF, Attawia M & Laurencin CT. Structural and human cellular assessment of a novel microsphere-based tissue engineered scaffolds for bone repair. Biomaterials 24, 597-609 (2003). 40. Oliveira SM et al. Characterization of polymeric solutions as injectable vehicles for hydroxyapatite microspheres. AAPS PharmSciTech 11, 852-858 (2010). 252 Dynamic In Vitro Characterization of Injectable Composite CPC Microcarriers 41. Matsuno T et al. Preparation of injectable 3D-formed β-tricalcium phosphate bead/alginate composite for bone tissue engineering. Dental Materials Journal 27, 827-834 (2008). 42. Hunt NC & Grover LM. Cell encapsulation using biopolymer gels for regnerative medicine. Biotechnology Letters 32, 733-742 (2010). 43. Trivedi N et al. Islets in alginate macrobeads reverse diabetes despite minimal acute insulin secretory responses. Transplantation 71, 203-211 (2001). 44. Park JK & Chang HN. Microencapsulation of microbial cells. Biotechnology Advances 18, 303-319 (2000). 45. Machida-Sano I, Matsuda Y & Namiki H. In vitro adhesion of human dermal fibroblasts on iron cross-linked alginate films. Biomedical Materials 4, 1-8 (2009). 46. Wang L et al. Evaluation of sodium alginate for bone marrow cell tissue engineering. Biomaterials 24, 3475-3481 (2003). 47. Becker TA, Kipke DR & Brandon T. Calcium alginate gel: a biocompatible and mechanically stable polymer for endovascular embolization. Journal of Biomedical Materials Research 54, 76-86 (2001). 48. Matthew IR, Browne RM, Frame JW & Millar BG. Subperiosteal behavior of alginate and cellulose wound dressing materials. Biomaterials 6, 275-278 (1995). 49. Iannuccelli V et al. Biodegradable intraoperative system for bone infection treatment 0.2. In vivo evaluation. International Journal of Pharmaceutics 143, 187-194 (1996). 50. Wu SF, Suzuki Y, Tanihara M, Ohniiahi K & Endo K Nishimura Y. Repair of facile nerve with alginate sponge without suturing: an experimental study in cats. Scandinavian journal of plastic reconstruction hand surgery 36, 135-140 (2002). Conclusions and future perspectives 253 Conclusions and Future Perspectives Conclusions Injectable Calcium phosphate cements with collagen 1. The injectable calcium phosphate with collagen in its liquid phase was successfully fabricated and characterized. 2. The presence of collagen in the CPC slightly delayed the initial hydrolysis of the α-TCP. The two main factors that determined this behavior were directly related with the acetic acid and to the higher viscosity of the collagen solution compared to water. 3. The analysis by XRD revealed the complete hydrolysis of α-TCP to CDHA in the presence of collagen, meaning that the reaction was not affected in terms of the final product. 4. During the setting reaction of the collagen-CPC in water, collagen was not released after 7 days, even if it was not crosslinked. 5. The initial conformation of collagen was controlled obtaining fibrillised and solubilized collagen. The distribution of this collagen in the CPC after the setting reaction was different depending on this initial collagen conformation, obtaining homogenous distribution for the solubilized collagen and heterogeneous distribution for the fibrillised collagen. 6. The presence of solubilized collagen increased the injectability of the paste. 7. Collagen did not affect the compressive strength of the CPC at low collagen concentrations (10 mg/ml), but as the collagen concentration was increased (50 mg/ml), the compressive strength was decreased. 8. Cell proliferation was enhanced in the presence of solubilized. ALP activity was high in the presence of the CPC. Collagen did not have a significant effect on ALP activity, although the ALP pattern changed, obtaining the maximum ALP value after 1 day, whereas in the absence of collagen, the maximum was obtained at 7 days. 254 Conclusions and future perspectives Collagen-Calcium phosphate cement scaffolds 1. Macroporous collagen scaffolds with increasing amounts of CPC were fabricated. The collagen scaffold served as a template for the CPC to deposit on top of it. 2. The transformation of α-TCP into CDHA took place inside the collagen matrix. 3. The scaffolds were able to sustain adhesion, proliferation and differentiation of mesenchymal stem cells. As the amount of CPC was increased, the proliferation initially decreased, whereas the ALP activity increased. 4. A plasmid encoding BMP7 was incorporated into the scaffolds and it resulted in an increase in cell number. The amount of BMP7 expressed was significant, but did not differ when changing the amount of plasmid incorporated. Calcium phosphate cement Microcarriers 1. Viable MC made of CPC mixed with collagen and gelatin were prepared. The size, shape and porosity were tailored by changing the composition of the CPC and the emulsion parameters, such as oil viscosity or agitation speed. 2. The presence of the biopolymers (collagen or gelatin) increased the sphericity of the MC. 3. The MC had a high porosity (∼60% depending on the MC composition), in a range of pore size between 0.5 and 5 µm, which would be useful for drug delivery applications. 4. Cells cultured on the MC showed a higher cell adhesion in the presence of gelatin compared to the rest of the materials, whereas after 14 days, collagen had the highest values of cell proliferation. 5. The dynamic culture of MC in spinner flasks allowed cell adhesion and proliferation of cells on the MC, having higher rates of proliferation compared to the static cultures. Future Perspectives The results obtained in the present thesis are promising in the field of tissue engineering and regenerative medicine. To be able to increase their potentially in this field, it would be of great interest to be able to incorporate some type of signaling to these CPC, such Conclusions and future perspectives 255 as antibiotics or drugs. This could enhance bone regeneration in the site of defect or prevent infections once implanted. Furthermore, in order to enhance the angiogenesis, the dense calcium phosphate cements could be prepared as macroporous in order to allow for blood vessels to penetrate the whole material. This could be done by foaming the liquid phase of the CPC, being collagen the liquid phase. Since collagen is a protein and presents amphiphilic properties, it has similar properties to surfactants and can therefore form stable foams that can then be mixed with the powder to form macroporous CPC foams. Regarding the work on macroporous scaffolds made of collagen and calcium phosphate cement and its use as gene delivery vehicle, they also showed promising results. In order to verify if these scaffolds would allow bone to grow ectopically, the scaffolds loaded with the BMP7 gene could be implanted in vivo in an animal model in order to observe if bone growth would take place outside of a bone region. Nevertheless, the efficiency of the plasmid incorporated as well as the amount of protein expressed need to be optimized. One of the approaches would be to further protect the gene inside the scaffold so that cells do not degrade the gene once it penetrates the cell membrane. For this purpose, the scaffold preparation can be modified, such as combining the gene with the CPC powder in order to obtain a paste slurry with gene and CPC, which would then be mixed with the collagen slurry to obtain a CPC/gene-collagen slurry, which upon the freeze-drying would give as a result the CPC-collagen scaffolds incorporating a gene in the matrix of the scaffold. Microcarriers would be the ideal candidate to be used as drug delivery system. These have demonstrated to have microporosity suitable for releasing antibiotics, drugs or growth factors. The advantage of using these CPC MC is that the drug could be delivered though two main systems, such as the incorporation in the CPC paste for a supposed long deliver, or can also be incorporated by adsorption on the MC. The release would depend on the microporosity of the MC, which can also be tailored according to the CPC formulation. Furthermore, cells could also be seeded on top of the MC as was observed, and the combination of the cells with osteogenic potential, with the osteoconductive calcium phosphate and a drug/growth factor with osteinductive potential, would lead to an ideal tissue engineering scaffold. An osteoinductive growth factor that could be used are those described in Chapter 4, being BMP-7 or BMP-2. 256 Conclusions and future perspectives Furthermore, even though these MC have already been implanted in vivo, it would also be interesting to implant these MC combined with cells, incorporating an osteoinductive signal such as the mentioned BMP-7 and inject them through minimally invasive surgery with the studied alginate gel. This would confirm the viability of this composite as a promising biomaterial for tissue regeneration.