scieee AI-readable full text Open interactive document viewer

Improvements in tribological and anticorrosion performance of porous Ti-6Al-4V via PEO coating

García Cabezón, Ana Cristina,Rodríguez Méndez, María Luz,Amigó Borrás, Vicente,Bayón, Raquel,Salvo Comino, Coral,García Hernández, Celia,Martín Pedrosa, Fernando

Abstract

Producción Científica

Full text

Friction 9(5): 1303–1318 (2021) ISSN 2223-7690 https://doi.org/10.1007/s40544-020-0480-2 CN 10-1237/TH RESEARCH ARTICLE Improvements in tribological and anticorrosion performance of porous Ti–6Al–4V via PEO coating C. Garcia-Cabezón1,2,*, M.L. Rodríguez-Méndez2,3, V. Amigó Borrás4, R. Bayón5, C. Salvo-Comino3, C. Garcia- Hernandez3, F.Martin-Pedrosa1,2 1 Materials Engineering, E.I.I., Universidad de Valladolid, Valladolid 47011, Spain 2 BioecoUVA Research Institute, Universidad de Valladolid, Valladolid 47011, Spain 3 Group UVASENS, Escuela de Ingenierías Industriales, Universidad de Valladolid, Valladolid 47011, Spain 4 Instituto de Tecnología de Materials,Univesitat Politécnica de Valencia, Valencia 46022, Spain 5 Tribology Unit, Fundación IK4-Tekniker, Eibar 20600, Spain Received: 10 March 2020 / Revised: 19 May 2020 / Accepted: 07 December 2020 © The author(s) 2020. Abstract: Medical implants manufactured using biomaterial Ti–6Al–4V exhibit some disadvantages. Its higher elastic modulus than that of natural bone can cause stress shielding problems. This can be avoided using Ti–6Al–4V with pores in the implant structure. However, poor corrosion and tribocorrosion behaviors are yielded because of the large area exposed to the medium. To mitigate both issues, coating technologies can be applied. The plasma electrolytic oxidation (PEO) process is a cost-effective process that has been used successfully in nonporous Ti alloys. In this study, two PEO coatings with different amounts of Ca/P are used. However, reports regarding their application in porous materials are scarce. The effects of PEO treatments on corrosion and tribocorrosion in Ti–6Al–4V powder metallurgy are analyzed herein. The porous materials provide an efficient surface for PEO coatings, as demonstrated via scanning electron microscopy (SEM) and atomic force microscopy (AFM), and the porosity of the substrates improved the adherence of the coatings. The corrosion resistance measured via electrochemical impedance spectroscopy confirmed the beneficial effect of the coatings, particularly for long exposure time. The lower roughness, small pore size, and more compact film observed in the PEO–Ca/P sample resulted in favorable tribological and corrosion properties. Keywords: Ti-based alloys; corrosion; tribocorrosion; surface modification 1 Introduction Ti–6Al–4V alloy and pure Ti are the most preferred substances for biomedical applications such as orthopedic prostheses and dental implants [1]. Their lower Young’s modulus, higher fatigue strength, better biocompatibility, and higher corrosion resistance compared with those of cobalt alloys or stainless steels justify their use as biomaterials. Powder metallurgy (PM) is a technology capable of reducing the processing cost of Ti complex shape devices owing to its advantages such as lower material losses, fewer machining steps, better dimensional precision, and higher surface finish [2, 3]. Although Ti alloys have a lower elastic modulus than other metallic metals, in the last decade, several failures in implants associated with stress shielding problems have been reported [4, 5]. Components manufactured via PM contain residual porosity, which can reduce the elasticity modulus and improve cell adhesion [6]; however, it can worsen the mechanical properties and reduce the corrosion resistance [2]. A method to improve the mechanical properties and resistance to corrosion and tribocorrosion of porous Ti alloys is by * Corresponding author: C. Garcia-Cabezón, E-mail: cr[email protected] 1304 Friction 9(5): 1303–1318 (2021) | https://mc03.manuscriptcentral.com/friction modifying their surfaces. The response of medical devices to the biological environment depends primarily on the surface characteristics of the material and often requires different properties of the surface and bulk. Hence, it is advisable to transform the surface of Ti alloys with a layer that improves biocompatibility [6]. Coating techniques for developing biologically active coatings such as laser surface treatment, ion implantation, electrodeposition [7], physical vapor deposition [8], and anodic oxidation via plasma electrolytic oxidation (PEO) have been used. The last technique has recently been used successfully in Ti alloys [9–12]. During PEO, metallic substrates are anodically polarized to high voltages above the dielectric breakdown, inducing the generation of short-lived plasma microdischarges on the substrate–surface– electrolyte interface [13–15]. By applying a positive voltage exceeding the dielectric breakdown of the oxide film, anodization occurs. During film growth, plasma microdischarges are continuously produced over the film’s surface, accompanied by gas evolution and entrapment into the material as well as discharge channels created during the electrochemical process, inducing the formation of oxide films with a porous morphology and rough topography. In addition, oxide films produced via PEO are generally characterized by the presence of different crystallographic phases of Ti oxide such as rutile and anatase, which confer properties such as high hardness and consequently improved tribological properties as well as increased corrosion protection. The chemical compositions of the oxide films depend significantly on the electrolyte composition used to treat them and in general, and the films present hydrophilic properties [16–18]. The composition and microstructure of the metallic substrate selected for PEO are vital to the properties of the oxide films generated. In addition, parameters such as anodic voltage, current density applied, electrolyte composition, and temperature are crucial processing variables that significantly affect the properties of the grown PEO oxide films [19, 20]. In recent studies that investigate the effects of substrates, electrolyte compositions, and current modes on the properties of PEO films for pure Ti [21–23] and Ti–6Al–4V [18, 19, 24, 25] have been analyzed. Corrosion resistance was one of the most important factors analyzed, indicating that improved corrosion resistance in NaCl or PBS was primarily determined by the composition, thickness, and density of the inner layer. Meanwhile, the type and concentration of electrolyte species affected the corrosion resistance as well. Therefore, many researchers have focused on the role of various electrolytes with elements such as Ca, P, Mg, Si, Zn, and Mn on Ti and Ti–6Al–4V. They demonstrated that the modified electrolytes provided higher resistance to corrosion and better osseointegration of dental implants [22, 26, 27]. PEO in porous Ti has been scarcely reported [28–31]. However, it demonstrates great potential in the surface engineering of porous materials for biomedical applications. Porosity may be advantageous to the growth of PEO coating and can result in enhanced corrosion resistance and mechanical/tribological properties. In this regard, Toptan et al. [31] recently investigated highly porous Ti samples and demonstrated that anodic oxidation treatment with Ca and P improved resistance to tribocorrosion in untreated samples, particularly for intermediate porosities. Therefore, this study was conducted to investigate the PEO of porous Ti–6Al–4V and the resulting coatings from the electrochemical perspective. It is noteworthy that Ti alloys present low wear properties [32]. This tribological behavior is characterized by heavy adhesive wear, high coefficient of friction, and poor abrasion resistance [33]. Furthermore, the contact of the biomaterial with saliva can induce corrosion. This electrochemical damage combined with the wear generated results in tribocorrosion, which is considered as one of the main causes of dental implant failures. The tribocorrosion behavior of Ti improved after PEO treatments; therefore, the PEO–Ti-treated samples exhibited higher corrosion resistance in artificial saliva (AS) than non-modified Ti [34]. In addition, better osseointegration or biocide properties can be obtained by adjusting the composition of the electrolyte [35]. Studies regarding the effect of PEO on the tribocorrosion behavior of porous materials in AS investigated via pin-on-disk wear testing have not been reported. Hence, the main objective of this study is to investigate the effect of PEO coatings on porous Ti–6Al–4V samples produced via PM in AS using electrochemical testing, considering issues that may Friction 9(5): 1303–1318 (2021) 1305 ∣www.Springer.com/journal/40544 | Friction http://friction.tsinghuajournals.com emerge when using them as dental implants. Two PEO electrolyte solutions with different Ca/P ratios were analyzed. The corrosion resistance was evaluated via impedance measurements, considering the effect of immersion time in simulated body fluids. The tribocorrosion behavior was evaluated via a pin-on- disk wear test in an AS solution. To interpret the electrochemical results, the microstructure and surface aspects were considered. 2 Experimental 2.1 Materials Disc specimens of Ti–6Al–4V (20 mm in diameter and 6 mm in thickness) were obtained by blending elemental powders supplied by Se-Jong Materials Co., Ltd. The elemental powders were mixed in a tubule (electrical tumbler mixer, Bioengineering Inversina 2L, Germany) for 30 min. The final composition of the powder mixture was 6.62% Al, 4.55% V, 0.55% maximum O, 0.3% maximum N, 0.5% maximum H, and Ti balance. The powder mixture was uniaxially compacted at 600 MPa using a cylindrical floating die. Sintering was performed in two stages. The first one involved a speed of 15 °C/min up to 780 °C to obtain a homogeneous temperature, where allotropic transformation occurred in the entire mass; whereas the second one involved heating at a speed of 7 °C/min up to 1,250 °C for 3 h. Subsequently, cooling was performed in the oven. The entire process was performed in a high vacuum (< 10–4 MPa). No lubricant was added because of the high reactivity of Ti. The porosity was investigated via image analysis. A commercial keronite equipment (20 kW AC power supply, KERONITE, KT 20–50, UK) was used to perform PEO treatments on disc samples made of Ti–6Al–4V alloy. An electrochemical cell with a capacity of 50 L was used, and the samples and stainless steel mesh were used as the anode and cathode, respectively. PEO was performed at 25 A/dm2 for 10 min. Two different aqueous electrolytes were employed to compare the effect of the electrolyte composition. One of them was the commercial Keronite Electrolyte 1003-01 for Ti and a custom-developed electrolyte comprising 0.35 M calcium acetate (calcium acetate hydrate, Scharlab, Spain) and 0.02 M β-glycerol phosphate (β-glycerol phosphate disodium salt pentahydrate, Scharlab, Spain) as sources of Ca and P, respectively. After the PEO, the disks were rinsed in deionized water and labeled as PEO and PEO–Ca/P, respectively. 2.2 Microstructural characterization The samples were investigated via optical metallography and scanning electron microscopy with energy dispersive X-ray spectroscopy (SEM/EDS) using an SEM instrument (QUANTA 200F, FEI). Kroll’s reagent (HNO3–HF–H2O) was used for 5 s of etching. Atomic force microscopy (AFM) images were recorded in a porous substrate and PEO-coated samples at room temperature in a Cypher ES (Asylum Instruments, USA) operated in the tapping mode. 2.3 Corrosion testing Electrochemical corrosion measurements were conducted using an impedance analyzer (Solartron SI 1260, Leicester, England) combined with an EG&G potentiostat. A conventional three-electrode cell was used. The counter electrode was a graphite rod, and the reference electrode was an Ag|AgCl/KCl saturated electrode. A physiological AS solution (2 g/L NaCl, 2 g/L KCl, 3.95 g/L CaCl2, 1.54 g/L NaH2PO4, 5 g/L urea, and 0.005 g/L, Na2S) at 37 ± 1 °C was used as the electrolyte. Electrochemical impedance spectroscopy (EIS) was performed, where impedance spectra were acquired in an AS solution at a frequency range from 1 MHz to 0.01 Hz and a signal amplitude of 10 mV at an open-circuit potential (OCP) before stabilization was performed for 1,800 s on the open circuit. Additionally, EIS analysis was performed on the samples after 15, 30, 45, 60, 75, and 90 days of immersion in the AS solution at 37 ± 1 °C. Impedance data were processed using Zview software and fitted to equivalent circuits. The tests were repeated thrice. 2.4 Tribocorrosion testing Pin-on-disk tribocorrosion tests were performed on a Microtest tribometer connected to an EG&G potentiostat using MT4002 software. The disk was connected as the operating electrode; the counter-electrode comprised 1306 Friction 9(5): 1303–1318 (2021) | https://mc03.manuscriptcentral.com/friction two graphite bars, and Ag/AgCl KCl 1M was used as the reference electrode. An electrochemical cell with the physiological AS solution at 37 ± 1 °C was connected to the tribometer. An alumina ball (3 mm in diameter and 1,500– 1,650 HV in Vickers hardness) was used as the counterbody. Prior to commencing the wear test, reference Ti–6Al–4V specimens were polished up to 1 μm diamond and cleaned in an ultrasonic bath. The PEO samples were ultrasonically cleaned only. OCP measurements were used as the tribocorrosion technique. The OCP was recorded against time throughout the pin-on-disk sliding tests. The coefficient of friction (COF), temperature, and track depth were continuously recorded. The evolution of the OCP was measured in the absence of loading, mechanical loading, and unloading. The potential was recorded for 1,800 s before starting the corrosion-wear sliding, which lasted for 3,600 s when a 4 N load was applied and 1,800 s after the load was removed. The disk was rotating at 60 rpm, whereas the sliding velocity and track radius were 0.1 m/s and 2 mm, respectively. All pin-on-disc tests were repeated thrice to ensure reproducibility. It is noteworthy that the aim of the tribocorrosion tests was not to simulate the real behavior of the materials as implants. Instead, it was performed to compare the different materials such that the most appropriate material can be identified. After the wear tests, the general characteristics of the wear track and the determination of the wear volume loss were evaluated using profilometry. The wear rate was calculated using Eq. (1), and the volume loss of wear was calculated based on the appendix of American Society for Testing and Materials (ASTM) G99-05 standard [36]. Worn surfaces were observed via SEM to identify the wear mechanisms.      311 3 Wear rate mm N m Volume loss (mm ) Normal load (N) Sliding distance (m) (1) 3 Results and discussion 3.1 Microstructural characterization A typical duplex lamellar α + β structure was observed in the Ti–6Al–4V sample sintered in a vacuum (Fig. 1(a)). The black areas shown correspond to pores. The average porosity of the samples was approximately 5.5 vol%, the average area of the pores was 54 μm2, and their average sphericity was 0.8. The average grain area was 185 μm2. All the parameters were determined using Buehler Omnimet image analysis. The X-ray diffraction (XRD) patterns of the substrate sample, as shown in Fig. 1(b), confirmed that α-Hexagonal close-Packed (HCP) was the main phase, and that a small amount of β-Body-centered cubic (BCC) phase retained at room temperature owing the presence of V as a beta stabilizer. Figure 1(c) depicts the SEM image of the substrate, showing the Fig. 1 (a) Light optical micrograph, (b) XRD diffractograms, and (c) SEM–BSE micrograph of porous Ti–6Al–4V. Friction 9(5): 1303–1318 (2021) 1307 ∣www.Springer.com/journal/40544 | Friction http://friction.tsinghuajournals.com lamellar constituent that is identified as a combination of the α-HCP phase (dark) and β-BCC phase (light), which retained in the form of thin plates. EDS confirmed that the β-BCC phase had a lower Al/V ratio (0.27) than the α-HCP phase (7.1). The mechanical properties of the porous Ti–6Al–4V substrate, such as the elasticity modulus and hardness, were measured. The microhardness, determined via the Vickers test using 0.3 kg for 10 s for the five samples, was 363.40 ± 30.96. The Vickers macrohardness (30 kg for 30 s) was 310 ± 19. As expected, the macrohardness value was slightly lower than that owing to the effect of porosity. The elasticity modulus of the porous Ti alloy, determined via ultrasonic testing, was 114.76 ± 1.66 GPa. The mechanical resistance and deformation of the substrate obtained via the three-point bending test were 1687.23 ± 90.2 MPa and 4.63 ± 0.29, respectively. Figures 2(a) and 2(b) show the surface morphologies of the coated samples corresponding to the PEO and PEO-Ca/P samples, respectively. Both samples exhibited a typical pancake shape structure with a regular and dispersed micropore network, although the PEO Ca/P sample showed a more uniform size and shape in the micropore structure. The cross section and thickness of the coated samples are depicted in Figs. 2(c) and 2(d), respectively, showing a more uniform and thinner inner layer as well as a more heterogeneous outer layer. The coating thickness was similar for both samples (approximately 16 μm). The most conspicuous difference between the two PEO samples was the chemical composition between the inner and outer layers, as shown in Table 1. For both samples, the amounts of metallic elements from the substrate, such as Ti, Al, and V, were higher in the inner layer, whereas the amounts of Ca, P, and Na were higher in the outer layer. The main differences between the PEO and PEO–Ca/P samples were the absence of V in the PEO coating sample and the highest [Ca]/[P] ratio in PEO–Ca/P. The ratio was approximately 1.5, which was similar to the case of natural bone in the PEO–Ca/P sample [27]. The above results reveal that both coatings have their own advantages. One of the main restrictions of the application of the alloy on bone implants is the release of toxic ions from the implant that can cause irritation to adjacent tissues. In this regard, the PEO Fig. 2 SEM images of Ti–6Al–4V surfaces subjected to PEO (a) superficial PEO sample, (b) superficial PEO–Ca/P sample, (c) cross section of PEO sample, and (d) cross section of PEO–Ca/P sample; (e) XRD diffractograms of coated samples. coating in which no vanadium is present may be more recommendable than the PEO–Ca/P coating [37]. In contrast, in the PEO–Ca/P coating, a higher amount of Ca and P has been detected, which would improve the biocompatibility of the titanium [38]. Figure 2(e) shows sharp peaks, indicating that the oxides formed contained crystalline and amorphous phases in addition to peaks corresponding to the substrate. The oxides formed in both samples were composed of rutile and anatase, the former being the dominant. It has been shown that anatase can improve the bioactivity, whereas rutile has a significantly higher hardness compared with anatase, affording improvement in the wear resistance [31, 34, 39]. Peaks of Ti, Na, and Ca complex phosphates were detected as well; however, they were difficult to be observed because some peaks coincided with those of the α-HCP 1308 Friction 9(5): 1303–1318 (2021) | https://mc03.manuscriptcentral.com/friction phase of Ti. The ratio of rutile to anatase was slightly higher in thePEO–Ca/P sample. The average roughness was similar for both PEO samples; however, a clear increase was observed with respect to the reference sample from 0.05 μm on the reference sample to 1.18 and 1.08 μm for the samples oxidized for PEO and PEO–Ca/P specimens, respectively. Additionally, the AFM topographic images of the substrate, as shown in Fig. 3(a), showed the flat structure of the metal alloy. The AFM images of the PEO-coated samples showed a non-uniform topographic surface with islands, as shown in Figs. 3(b) and 3(c). In the case of PEO–Ca/P, as shown in Fig. 3(b), more uniform and small individual grains were observed, and the pores and cracks had lower depths than those of the PEO sample (Fig. 3(c)). The root mean square roughness of the PEO sample was approximately 306 nm, whereas the roughness of the PEO–Ca/P sample was approximately 257 nm. The individual grains of the PEO sample had an average Table 1 EDS of PEO-treated Ti–6Al–4V alloy. Sample Zone Al (wt%) Ca (wt%) K (wt%) Na (wt%) P (wt%) Si (wt%) O (wt%) V (wt%) Ti (wt%) 1 2.91 0.66 0.16 0.33 4.68 0.46 45.62 — 45.44 PEO 2 3.25 0.45 0.14 0.30 4.20 0.35 43.21 — 48.14 1 3.51 5.62 0.28 1.25 5.04 0.35 38.00 1.96 43.99 PEO–Ca/P 2 3.82 5.93 0.29 1.22 3.99 0.21 37.51 2.02 44.76 Fig. 3 (a) AFM topographic images of Ti–6A–l4V substrate, (b) PEO coated sample, and (c) PEO–Ca/P-coated sample. Friction 9(5): 1303–1318 (2021) 1309 ∣www.Springer.com/journal/40544 | Friction http://friction.tsinghuajournals.com diameter of 400–500 nm, whereas the smallest grains measuring 200–300 nm were observed in the PEO–Ca/P sample. The line profile shows the importance of the pore depth and cracks. The depth and size of the pores of the PEO–Ca/P sample were smaller than those of the PEO sample. The lower roughness value, small grain size, small size, and number of pores in the PEO–Ca/P sample indicate that the coating was smoother and more compact with fewer pores compared with the PEO sample. This revealed that the electrolyte composition significantly affected the coating topography. The increased surface roughness achieved via these treatments can provide a stable bone-implant interface and promote the osseointegration of Ti implants [40]. 3.2 Corrosion behavior Impedance spectra can provide information regarding physicochemical processes occurring in the Ti–6Al–4V alloy and PEO-coated samples while they were corroding in the AS solution. The Bode and Nyquist diagrams for the reference sample at different immersion time (0, 15, 30, 45, 60, 75, and 90 days) in the simulated fluid (AS) at an OCP are presented in Fig. 4. The Nyquist curves revealed an incomplete capacitive loop. The semicircle increased in radius when the exposition time increased. Considering that a larger semicircle radius results in greater resistance to polarization in the material, it can be concluded that corrosion resistance increased during exposure. The impedance modulus was more than one order of magnitude higher for the sample measured after 90 days of exposure compared with that of the initial testing sample, indicating the better corrosion behavior of the former. The double layer and oxide capacitances were related to the dependence of the frequency on the phase angle. This increase in the corrosion resistance of non-modified Ti–6Al–4V with exposure time is attributed to the development of a reconstructed and thickened passive layer. This enhanced passive film is observed in conventional [21] and PM [5] Ti alloys. The effect of immersion time in the aggressive solution for the PEO-coated samples differed from that for the noncoated sample but similar for both coatings. As shown in the Bode diagrams, the most significant changes occurred after 15 and 30 days of immersion, and the prolonged exposure time resulted in a slight increase and decrease in the impedance module without significant changes in the spectra. For the PEO-coated sample, the exposition in AS resulted in an increase in the impedance module, particularly at high and medium frequencies, as shown in Fig. 5(a); meanwhile, for the PEO–Ca/P-coated sample, the increase occurred in all frequency ranges, as shown in Fig. 5(b). For comparison, Fig. 6 presents the Nyquist and Bode diagrams of the EIS results obtained for Ti–6Al–4V with and without PEO coating. Figure 6(a) shows the equivalent electric circuit proposed to interpret the EIS spectra of the uncoated and coated samples. Furthermore, Fig. 6 graphically shows the results of the fittings for 0 (Figs. 6(b)–6(d)) and 90 days (Figs. 6(e)–6(g)) of immersion time in AS. The beneficial effect of the coating is clear before and after the immersion of the samples. Both PEO-coated samples showed a clear increase in the impedance module at all frequencies with the increase in the radius of Fig. 4 Effect of immersion time in AS solution on EIS depicted in (a) Nyquist and (b, c) Bode plots of uncoated Ti–6Al–4 V sample. 1310 Friction 9(5): 1303–1318 (2021) | https://mc03.manuscriptcentral.com/friction Fig. 5 Effect of immersion time in AS solution on Bode plots of (a) PEO-coated and (b) PEO–Ca/P-coated samples. Fig. 6 Nyquist and Bode plots of Ti–6Al–4V, PEO, and PEO–Ca/P samples in AS solution after: (a–c) 0 days and (d–f) 90 days o f immersion. (g) Results of fitting to equivalent electric circuit are included. Friction 9(5): 1303–1318 (2021) 1311 ∣www.Springer.com/journal/40544 | Friction http://friction.tsinghuajournals.com the depressed circle shown in the Nyquist plot. The PEO–Ca/P sample showed the highest impedance module before and after immersion in AS. The Bode diagrams indicate that the uncoated Ti–6Al–4V presented a stable passive film on the surface, considering the capacitance and phase angle of ~90° in the low–middle frequency range. The PEO-coated sample appeared to generate the same pattern, but in the PEO–Ca/P-coated sample, the angle was reduced from 50° to 20° in the mid–high frequency range. The different corrosion behaviors with exposure time for the uncoated and coated samples may be related to the nature of the oxide film. The spontaneous passivating oxide present on the uncoated samples was polycrystalline and exhibited severe pitting and crevice corrosion [41], whereas surface treatment for forming an amorphous oxide resulted in excellent corrosion resistance [42]. Table 2 lists the parameters of the fitting. Chi-square values, χ2, were used to evaluate the quality of the fittings. The variable χ2 was on the order of 10−4. In the proposed model for the noncoated sample, CPE1 is the first time constant represented by the capacitance of the passive film in pore-free areas, and R1 is the resistance of the porous oxide passive layer impregnated with the electrolyte. The electrolyte can penetrate through the pores of the passive layer. These defects resulted in the appearance of a second time constant related to the dissolution of the metal due to the formation of a nonprotective passive layer. Therefore, this second time constant may indicate that the substrate below the defective passive layer was subjected to a rapid dissolution process. The variables CPE2 and R2 can be associated with the charge-transfer process through the nonprotected passive layer. These pores resulted in a double-layer capacitance (CPE2) and a charge-transfer resistance (R2). A similar equivalent electric circuit was used to analyze the corrosion mechanism of porous Ti–6Al–4V alloy in physiological solutions [5] and other porous passive materials [43]. The porosity of the Ti–6Al–4V alloy resulted in a lower corrosion resistance value (R1 + R2) compared with those of solid alloys [44], resulting in a higher susceptibility of the porous materials to local corrosion. It was assumed that the relatively small pores in the cell walls favored the placement of electrolytes and oxygen depletion. This is vital to the stability and preservation of the Ti oxide layer; hence, the low resistance and high capacitance values were obtained from the uncoated sample. For the coated samples, CPE1 and R1 were related to the high frequency constant associated with the porous outer layer of the PEO coating, whereas CPE2 and R2 were related to the medium-frequency time constant corresponding to the more compact inner layer of the PEO coating. An additional resistive Warburg element appeared in the PEO coating samples, reflecting a case of control by diffusion in the electrolyte or in a surface coating. This equivalent circuit has been used for nonporous PEO-coated samples [22]. The CPE element was used instead of the typical ideal capacitor, as indicated by the depressed circle observed in the Nyquist diagram. The impedance of this element is expressed as follows:   CPE 1 (j )n ZC (2) where j is the imaginary unit. When n = 1, the CPE is an ideal capacitor; when n = 0, it describes an ideal resistor; and when n = –1, it is a pure inductance; furthermore, C is a constant. As mentioned previously, Table 2 EIS equivalent circuit parameters of reference and coated samples. Sample Time (d) CPE1–C (10−6 sn·Ω−1·cm−2) CPE1–n R1 (Ω·cm−2) CPEC2–C (10−6 sn·Ω−1·cm−2)CPE2–n R2 (Ω·cm−2) χ2 (10−4) 0 20.1 0.29 152.1 13.2 0.86 46,985 5 Ti–6Al–4V 90 4.71 0.39 80.9 11.0 0.87 5.92×1015 8.3 0 5.67 0.76 8,405 0.004 0.79 730,540 9 PEO 90 1.01 0.65 4,202 7.22 0.50 8.76×1019 2 0 36.6 0.42 2,504 0.04 0.86 35469 2 PEO–Ca/P 90 1.89 0.27 5.886 0.07 0.72 7.15×1019 8 1318 Friction 9(5): 1303–1318 (2021) | https://mc03.manuscriptcentral.com/friction Ti6Al4V alloy in alkaline solutions. Tribol Int 128: 1–8 (2018) [54] Laurindo C A H, Lepienski C M, Amorim F L, Torres R D, Soares P. Mechanical and tribological properties of Ca/P-doped titanium dioxide layer produced by plasma electrolytic oxidation: Effects of applied voltage and heat treatment. Tribol Trans 61(4): 733–741 (2018) [55] Kikuchi M, Takahashi M, Okuno O. Elastic moduli of cast Ti–Au, Ti–Ag, and Ti–Cu alloys. Dent Mater 22(7): 641–646 (2006) [56] Niinomi M, Akahori T, Takeuchi T, Katsura S, Fukui H, Toda H. Mechanical properties and cyto-toxicity of new beta type titanium alloy with low melting points for dental applications. Mater Sci Eng: C 25(3): 417–425 (2005) Cristina García Cabezón. She is a professor at the Engineers School of the University of Valladolid and and the co-head of the group UVASens, dedicated to the development of electrochemical sensors for the analysis of foods. She obtained a B.S.C. degree in Chemistry (U. Zaragoza, 1991) and obtained her Ph.D. degree in industrial engineering from the University of Valladolid (1998) where she is currently a professor at the Department of Materials Science. For several years, her research was dedicated to the study of the electrochemical behavior of metals and metal nanoparticles and she became an expert in electrochemistry. Her investigation in the field of materials science and engineering is focused on corrosion, porous materials, and coatings. The materials in which these studies have been carried out are stainless steels, cobalt alloys, and titanium alloys. In 2010, she joined the group UVASens, dedicated to the development of electrochemical sensors for the analysis of foods, where her skills in electrochemistry of metals and nanoparticles busted the research in the field of electronic tongues of the group. She has developed electrochemical sensors based on nanoparticles dedicated to the detection of antioxidants and the analysis in wines and milks. She is an author or co-author of 54 indexed articles (h-index 15). She has colaborations with several national and international groups. In particular, she is directing the collaboration with the group of Sensors of the I.P. Braganza (Portugal). She serves a referee of several journals related to electrochemistry (electrochimica acta, corrosion science, sensors, etc.). She reviews 12–15 papers per year. She regularly participates in contracts with industries.