scieee AI-readable full text Open interactive document viewer

Study of steam explosion pretreatment and preservation methods of commercial cellulose

Lorenzo Hernando, Ana María,Martín Juarez, Judit,Bolado Rodríguez, Silvia

Abstract

UIC-Consejería de Educación Junta de Castilla y León, University of Valladolid

Full text

1 Study of steam explosion pretreatment and preservation methods of commercial cellulose Ana Lorenzo Hernando a, Judit Martín Juárez a, Silvia Bolado Rodríguez a* a Department of Chemical Engineering and Environmental Technology, University of Valladolid, Calle Doctor Mergelina s/n, 47011, Valladolid, Spain E-mails: [email protected]; [email protected]; [email protected] *Corresponding author Highlights Steam explosion is a promising pre-treatment for compact cellulose Treatment at 150ºC reduced crystallinity, but at 200ºC favoured recrystallization Despite polymerization reduction, steam explosion reduced enzymatic accessibility Acetone counteracted crystallinity and accessibility changes and reduced viscosity Freezing caused severe degradative effects in accessibility and crystallinity ACCEPTED MANUSCRIPT 2 Abstract Steam explosion (150 – 200 ºC, 5 – 30 min) was performed on a commercial cellulose presented in two configurations (fiberized and compact sheet) and its effect on their chemical and physical properties was studied, along with the influence of two different preservation methods (acetone drying and freezing) after pretreatment. No degradation compounds were produced during pretreatment, although solid recovery (RS) decreased with temperature from 90% to 62%. Similar particle size and surface conditions (increased porosity) were found for both types of pretreated samples despite the extremely different initial configuration. Crystallinity diminished for 150 ºC samples, but 200 ºC pretreatment promoted recrystallization. Pretreatment also reduced polymerization degree, although enzymatic accessibility did not improve. Both acetone and freezing processes extremely affected cellulose properties. Acetone drying counterbalanced crystallinity and enzymatic accessibility variations of pretreated samples, while decreasing polymerization degree to 302. Freezing dramatically decreased enzymatic accessibility of pretreated samples down to 15.8%. Keywords Natural fiber, crystallinity, enzymatic hydrolysis, degree of polymerization, acetone drying, freezing. ACCEPTED MANUSCRIPT 3 1. Introduction Fossil sources depletion has increased prices of petrol-derived polymers and natural fibers are starting to be considered a suitable alternative due to their easy processing and eco-friendly advantages. Significant amounts of natural fibers are currently considered a waste, and their disposal creates harmful environmental problems (Oliveira et al., 2013), so they can be a promising renewable raw material due to their abundance and low cost. Among the new alternative uses, polymeric materials based on natural fibers are emerging in the last decades for numerous diary and important purposes, such in biomedical or automotive industries (Thakur & Thakur, 2014). Natural fibers are a well-known source of cellulose, since it is its principal component (≥ 60%). Usually, chemical methods are used to produce cellulose rich pulp, which is commercialized as roll-sheets of compacted fibers, being transformed back into fibers by mechanical processes such as carding. A pretreatment like steam explosion could be a useful step in cellulose production processes for both substituting physical opening of cellulose rolls and improving cellulose fibers versatility, opening its structure and increasing its porosity, reactivity and specific surface, with minimum degradation. It is an innovative and effective pretreatment which has provided interesting results for lignocellulosic biomass. It consists in applying highpressure saturated steam to biomass for short times, followed by a sudden decompression. Its advantages over chemical methods are low environmental impact and capital investment, energy efficiency, and the possibility of treating larger amounts of biomass (Jacquet et al., 2012). Commonly, steam explosion processes take place at temperatures between 150 ºC and 250 ºC for times varying from 2 to 60 min. Severity factor (SF) of the process is calculated from these two variables by Eq. 1 (Jacquet et al., 2011): ACCEPTED MANUSCRIPT 4 SF = log10 [tSE* exp ( (T-100) 14.75) ⁄ ] (1) Where tSE is reaction time (min) and T is the steam temperature (°C). The steam breaks and modifies the structure and could even provoke the hydrolysis of the glycosidic bonds, producing organic acids due to shearing forces during decompression (Medina et al., 2016). The global effect of both processes involves modifications on physical and chemical properties of the biomass such as reactivity (related with specific surface area), viscosity or crystallinity among others (Sui & Chen, 2016), which can be beneficial for ulterior industrial uses of cellulose fibers. When applied to lignocellulosic materials, steam explosion treatment lead to opened structures, modification of physicochemical properties such as the specific surface area, depolymerization and solubilization of hemicellulose, and increase of cellulose enzymatic hydrolysis degree, assisting following valorization processes. (Medina et al., 2016; Neves, Pitarelo, & Ramos, 2016), However, scarce information about its effects on commercial cellulose fibers could be found. (Jacquet et al., 2011) studied the effect of different conditions during the steam explosion on degradation of pure cellulose, finding degradation products as 5- hydroxymethyl furfural (HMF) for severity factors higher than 4.0. In their subsequent study, (Jacquet et al., 2012) reported no improvement on enzymatic hydrolysis rate after steam explosion. Nevertheless, they observed modification on physicochemical properties of cellulose fibers, such as an increase in water retention and crystallinity index values. Water retention after treatment might play a significant role not only during pretreatment but afterwards as well, even accelerating cellulose degradation (Sui & Chen, 2016). (Yamashiki et al., 1990) used acetone instead of the traditional oven drying, to avoid drastic structural changes due to temperature. Nevertheless, they did not consider ACCEPTED MANUSCRIPT 5 that acetone might also have some other effects. After drying, samples are usually stored in -20 ºC freezers, but the formation of ice crystallites might harm microfibrils structure. To the best of authors’ knowledge, no study has been conducted for systematically evaluating the influence of steam explosion in compacted cellulose pulps or the influence of the preservation methods on physical properties. The aim of this work was to study steam explosion as a pretreatment for commercial cellulose samples presented in two different handlings, to explore the possibilities of this treatment as a substitute for other mechanical pretreatments and its effects on the modification of several physicochemical properties of cellulose fibers regarding a future use. To that end, several analyses were performed such as chemical composition, particle size distribution, crystallinity rate, limiting viscosity number and degree of polymerization. In addition, two different preservation methods of pretreated samples (acetone washing and freezing) were tested to study the effects of preservation methods could have on the stability and quality of pretreated samples. 2. Materials and methods 2.1. Raw material One bleached commercial cellulose was used in this work, obtained 100% from softwoods pulp, purified from lignin and hemicellulose and presented in two different handlings: Compacted Cellulose (CC) was provided as a compacted sheet and cut in small squared pieces (10x30mm approx.) for better manipulation. Fiberized Cellulose (FC) was obtained by mechanical fiberization of the sheet. Chemical composition (moisture, cellulose, hemicellulose, lignin, extractives and ash content), particle size distribution, enzymatic hydrolysis kinetics, optical an electronic ACCEPTED MANUSCRIPT 6 scanning microscopy analysis, soluble impurities (short-chain organic acids, HMF, furfural, and phenols), crystallinity index and limiting viscosity number were analyzed. 2.2. Steam explosion experiments Steam explosion experiments were conducted in a 5L stainless-steel reactor, connected on top to a steam generator. Reactor bottom discharged through an electrovalve to a flash vessel partially open to the atmosphere. The reactor was loaded with 50.0 g of cellulose, tightly closed and filled with saturated steam at the desired temperature and pressure. After reaching experimental conditions (this period was called “demand time”, td), a countdown for the defined reaction time (tSE) started. Once it finished, the bottom electrovalve automatically opened, discharging the reactor content into the flash vessel. A set of four experiments was conducted for each sample, combination of two reaction temperatures (150 or 200 ºC) and two reaction times (5 or 30min). Resulting pretreated cellulose was vacuum-filtrated in a Buchner funnel to eliminate excess water, weighed and stored in plastic flasks at 4 ºC before analysis. Samples of pretreatment liquid fraction were also stored for chemical analysis to determine possible solubilization and degradation due to pretreatment. The term “Severity Factor” (SF), calculated by Eq. (1), defined the intensity of the pretreatment, and the term “Solids recovery” (RS) provided the mass losses due to treatment or manipulation, referred to the initial amount of raw material. Due to the configuration of the steam explosion system, td never exceeded 100 seconds, and it has not been considered for SF calculations. Solids recovery (w/w %) was calculated through the ratio of the recovered and initially loaded mass, both in dry-matter base. ACCEPTED MANUSCRIPT 7 Pretreated samples were analyzed for chemical composition, particle size distribution, enzymatic hydrolysis kinetics, optical microscopy, crystallinity index, limiting viscosity number, and SEM. 2.3. Preservation methods assays Two different preservation methods were evaluated: (1) acetone-drying step and (2) freezing at -20 ºC. For (1), samples were profusely washed with acetone after filtration. Then, acetone-washed cellulose was dried for 48h at room temperature and stored in plastic flasks. Chemical composition, enzymatic hydrolysis kinetics, optical microscopy, crystallinity index and limiting viscosity number were conducted to evaluate composition and structural changes caused by acetone wash. For (2), pretreated samples were frozen at -20 ºC for 24h after water removal by filtration. After that time, they were defrosted and analyzed (chemical composition, enzymatic hydrolysis kinetics, optical microscopy and crystallinity index). 2.4. Physicochemical characterization 2.4.1. Chemical characterization The chemical composition analysis procedures followed NREL (National Renewable Energy Laboratory – USA) analytical procedures (TP-510-42618). Total and volatile solids (TS/VS), moisture, water extractives and ashes content were determined by gravimetric analysis. Cellulose and hemicellulose content were determined by HPLC analysis of acid hydrolysis liquid phase of samples. A Bio-Rad HPX-87H ion-exclusion column installed in a Waters e2695 separation module equipped with Waters 2414 refractive index detector was used to quantify the concentration of glucose. The mobile phase of 0.025 M H2SO4 was eluted at a flow ratio of 0.6 mL/min and 50 ºC. CC samples ACCEPTED MANUSCRIPT 8 needed three successive acid hydrolysis for their correct characterization. Acid Soluble Lignin (ASL) was determined by spectrophotometric method and Acid Insoluble Lignin (AIL) gravimetrically after acid hydrolysis of the samples. All results correspond to the mean value of two measures (Travaini, Barrado, & Bolado, 2016). Solubilized sugars and soluble impurities (HMF, furfural and short-chain organic acids) were determined by HPLC analysis of the liquid fraction of a cellulose-in-water suspension (at 1 g/L under continuous stirring for 24h), using the same conditions as previously indicated. Results correspond to the mean of two measures. Total phenolic content (TPC) were determined by spectrophotometric method at a wavelength of 765 nm according to an internal protocol of the Laboratory of Instrumental Analysis of University of Valladolid, based on the Folin reaction (Toquero & Bolado, 2014). 2.4.2. Physical characterization Particle size distribution was determined in triplicate on cellulose-in-water suspensions by Dynamic Laser Scattering (DLS) using a Mastersizer 2000 (Malvern Instruments Ltd), with an initial obscuration of 5%. This instrument reports particle size as a volume equivalent sphere diameter. While this is not an absolute measure, given that the fibre thickness can be considered uniform, it gives a relative value about the effect of the pre-treatment on the fibre length. Percentiles dp10 (equal to the value below which 10% of the observations may be found) and dp90 (equal to the value below which 90% of the observations may be found) were obtained, as well as particle size of the peaks. Optical microscopy was conducted with a Leica optical microscope at 100, 200 and 400 magnifications. Scanning Electron Microscopy was performed according to internal procedures, for magnifications from 70 to 30000. ACCEPTED MANUSCRIPT 9 Crystallinity index (ICr) was studied by X-ray diffraction (angular interval from 10º to 40º, 0.05 of path). ICr was calculated through the ratio of intensities Iam (minimum intensity in 2θ between 18º and 19º) and I002 (maximum intensity of the crystalline peak in 2θ between 22º and 23º) (Buschle‐Diller & Zeronian, 1992). Limiting viscosity number ([η]) was measured in triplicate according to ISO 5351:2012, using a Cannon-Fenske viscometer. Cellulose samples were dissolved in 0.5M cupriethylenediamine solution at 0.003 g/mL and agitated for 30 minutes before solution viscosity was recorded. The degree of polymerization (DP) of samples was estimated using Immergut’s equation (Immergut, Ranby, & Mark, 1953). DP0.905 = 0.805*[η] (2) 2.4.3. Enzymatic hydrolysis kinetics Enzymatic hydrolysis was conducted using a commercial enzymatic cocktail kindly provided by Novozymes©, with a dosage of 10 FPU/g (Celluclast 1.5L, cellulase from Trichoderma reseii) and 40 CBU/g (Novozyme 188), performed at 50 ºC using 3% (w/w dry-matter base) cellulose suspensions for 48h. pH was adjusted at 4.9 with 5mM sodium acetate buffer (Travaini, Barrado, & Bolado-Rodríguez, 2016). Experimental time courses of glucose release were tracked every 4 hours, and glucose concentration was measured by HPLC as reported. Considering prior work, these values were fitted according to a single hyperbola (Nidetzky, Steiner, Hayn, & Esterbauer, 1993): XG=at (b+t) ⁄ (3) where XG is the degree of cellulose hydrolysis (% w/w of cellulose), a and b factors describing cellulose hydrolysis kinetics, and t is time (h). Criteria for selecting the model for curve fitting were the sum of least squares, mean square error, and normal distribution of residuals. Kinetic factors were obtained through curve fitting of cellulose ACCEPTED MANUSCRIPT 16 Fig. 2. Crystallinity index. Crystallinity index (ICr) obtained from X-ray spectrometry of samples before (raw material (‒ · ‒)) and after steam explosion (FC (●), CC (○)); and after acetone drying (DFC (■), DCC (□)) or freezing process (FFC (▲), FCC (∆)) as a function of the severity factor. X-ray patterns of all samples corresponded to typical crystalline structure of raw cellulose. The presence of crystalline fraction was corroborated with the moderately high values (around 3.0) of the ratio between intensities at 22.7 º and 20.4 º, which indicates the relative proportion between types of cellulose I and II. Pretreatment at 150 ºC decreased ICr of samples, being the greatest reduction compared to raw material (8 percentage points) for pretreated FC. However, 200 ºC steam explosions did not significantly modify ICr, with maximum ICr value of 82.2% for sample CC10. These results could indicate that steam explosion reduced the crystalline fraction, but hightemperature (and hence higher pressure) treatment promoted recrystallization, partially cancelling out or exceeding the downgrading effect. Some protective effect of compact configuration could be observed, which is not effective at the most severe conditions. Reaction time was only significant at high temperature experiments. (Wang, Jiang, Xu, & Sun, 2009) did not find significant variation on microcrystalline structure of Lespedeza fibers even at the most severe conditions. Differently, limiting viscosity number (and hence the degree of polymerization) of pretreated samples decreased for all the fiberized samples to values ranging from 480 to 660 mL/g, and showing this time a greater influence of pretreatment time than that of temperature (Fig. 3). ACCEPTED MANUSCRIPT 17 Fig. 3. Limiting viscosity number. Limiting viscosity number ([η]) of samples before (raw material (‒ · ‒)) and after steam explosion treatment (FC (●), CC (○)); and after acetone drying (DFC (■), DCC (□)) as a function of the severity factor. In the case of CC samples, 150 ºC pretreatments did not influence [η] and, so, polymerization of cellulose. The compactness of CC configuration provided a certain protection to cellulose polymer when working at low SFs. Nevertheless, at 200 ºC both FC and CC samples showed equivalent behavior, reaching similar [η] values. This dependence with severity factor was also observed by (Yamashiki et al., 1990), who reported a combined effect of temperature and time in degree of polymerization, but in this case applying severity factors over 4.45. They also reported a reduction in degree of polymerization as well as a shortening effect for steam-exploded cellulose fibers with temperatures below 230 ºC. 3.2.3. Enzymatic hydrolysis ACCEPTED MANUSCRIPT 18 Table 1 shows the fitted parameters of enzymatic hydrolysis kinetics of FC and CC cellulose pretreated samples applying (Eq. 3), and cellulose hydrolysis courses with time are shown in Figs. 4a and b. Fig. 4a and b. Enzymatic kinetics of raw and exploded materials. Enzymatic hydrolysis kinetics of raw cellulose and steam exploded samples of both fiberized (up) and compacted (down) handling celluloses. ACCEPTED MANUSCRIPT 19 Experimental results are shown as discrete points, lines represent the theoretical model of eq. 3 using the fitting parameters on Table 1. As before, CC and FC-exploded samples showed an analogous behavior and similar reaction courses, accessibilities (a) and kinetic parameters (k). Enzymatic hydrolysis of pretreated samples provided lower degree of hydrolysis of cellulose than raw materials, but increasing with the pretreatment temperature. On the other hand, the pretreatment reaction time had not a decisive effect. For all samples, 48h of enzymatic hydrolysis was enough to achieve the maximum liberation of the accessible cellulose in samples. Cellulose degree of hydrolysis at 48h were almost up to accessibility (a) values, being slightly higher for compact samples than for fiberized ones. Nevertheless, a clear reduction on accessibility was observed, represented by a generalized decrease in hydrolysis efficiency. This decrease was especially remarkable for low-temperature pretreated samples, increasing for 200 ºC experiments but never reaching the values obtained for raw materials. The evolution trend of both accessibility and ICr is very similar with increasing SF, suggesting a correlation between these two properties. Kinetic parameter (k) showed an opposite trend to accessibility. Enzymatic hydrolysis rate was high for low temperature pretreated samples, but 200 ºC pretreatments returned similar k values to those from the raw materials. The results shown no influence of pretreatment reaction time, with identical fitting parameter values for each sample configuration and temperature. This increase in k values could mean that, even if enzyme action was limited, the accessible cellulose was likely to be hydrolyzed, suggesting that steam explosion probably modified internal porosity and structure without extremely changing fiber physical properties. 3.3. Preservation methods study ACCEPTED MANUSCRIPT 20 The influence of acetone drying (samples called DFC and DCC) and freezing (FFC and FCC) and their effect on physical and chemical properties of pretreated cellulose were evaluated. 3.3.1. Acetone-dried preservation Chemical composition of acetone-dried samples remained almost unchanged, obtaining comparable values (data not shown) to pretreated samples from section 3.2. Acetone effectively dried steam-exploded samples for experiments conducted at 150 ºC of temperature for both compacted and fiberized pretreated samples, obtaining moisture values around 5%. Acetone-dried samples from 200 ºC pretreatments still retained notable amounts of water, observing significant variations depending on sample configuration and reaction time: moisture oscillated from 17.3 for DCC10 sample to 30.5% for DFC11. This significant water retention in 200 ºC pretreated samples could be related with the higher accessibility found for enzymatic hydrolysis of these samples. Optical microscopy images did not reveal significant changes on acetone-dried pretreated cellulose fibers. Surface appearance was similar to pretreated samples from section 3.2 (increased number and size of pores) but fibers were flat and more crumpled after acetone drying process. Surprisingly, acetone counterbalanced the variations of crystallinity index caused by steam explosion on pretreated samples (section 3.2) (Fig. 2). Crystallinity index of samples pretreated at low SFs, where ICr was reduced (FC00, FC01, FC10, CC00 and CC01), increased after acetone washing, and vice versa. This suggested that samples that recrystallized after 200ºC treatment might suffer a rearrangement during acetone drying, losing crystallinity. In addition, retained water might have an effect, i.e. polymeric chains from samples with higher moisture had more flexibility and presented less crystallinity. ACCEPTED MANUSCRIPT 21 On the other hand, limiting viscosity number was considerably reduced by acetone washing, obtaining a maximum [η] value of 540 mL/g and a minimum of 200 mL/g (Fig. 3) but with no clear dependence on pretreatment conditions. Thus, polymerization degrees (from Eq. 2) ranged from 818 to 302. These results indicated that acetone did not just remove inner water but also affected the structure of cellulose polymeric chains, probably due to a complex interaction between several properties of pretreated cellulose samples, like structure, polymerization degree or moisture content. Table 2. Enzymatic hydrolysis of preserved samples. Enzymatic kinetic parameters (accessibility a (%), kinetic coefficient k (h-1), and regression coefficient R2) of pretreated samples after acetone drying (DFCij, DCCij) and pretreated samples after freezing (FFCij, FCCij) DFC00 DFC01 DFC10 DFC11 DCC00 DCC01 DCC10 DCC11 a (%) 72.2 71.1 45.8 42.0 75.2 73.9 51.5 44.4 k (h-1) 0.083 0.083 0.172 0.172 0.095 0.095 0.192 0.192 R2 0.986 0.991 0.957 0.963 0.983 0.965 0.969 0.982 FFC00 FFC01 FFC10 FFC11 FCC00 FCC01 FCC10 FCC11 a (%) 21.4 15.8 22.0 17.6 30.8 21.36 31.6 23.0 k (h-1) 0.166 0.272 0.166 0.272 0.135 0.199 0.135 0.199 R2 0.946 0.944 0.981 0.964 0.977 0.936 0.983 0.976 ACCEPTED MANUSCRIPT 22 Fig. 5a and b. Enzymatic kinetics of acetone dried samples. Enzymatic hydrolysis kinetics of steam explosion pretreated samples of both fiberized (up) and compacted (down) handling celluloses, after acetone drying process. Experimental results are shown as discrete points, lines represent the theoretical model of equation 3 using the fitting parameters of Table 2. Enzymatic hydrolysis kinetics showed identical counterbalance effect as observed for ICr (Fig. 5). Acetone wash increased XG of samples pretreated at 150 ºC, but still not reaching raw cellulose results, and decreased for 200 ºC pretreated samples (Table 2). As observed in section 3.2, hydrolysis extension was softly higher in CC samples than in FC samples, even after acetone drying. On the other hand, kinetic parameter k was remarkably affected, increasing as accessibility decreased. Again, results showed no influence of reaction time, with identical fitting parameter values for each sample configuration and temperature. 3.3.2. Freeze preservation ACCEPTED MANUSCRIPT 23 Chemical composition did not show changes due to freezing (data not shown), but the rest of the properties were indeed affected, as it was also observed for acetone-dried samples. All frozen pretreated samples showed lower ICr values than for non-treated cellulose, decreasing between 3.0 (FCC00) and 9.2 (FFC11) percentage points compared to raw cellulose. Compared to pretreated samples, only ICr of FFC00, FFC10 and FCC00 samples (corresponding to low SFs) slightly increased, around 3 percentage points by freezing. Maximum decrease was observed for samples from high SFs pretreatments, those which suffer recrystallization, with ICr reductions down to 10 percentage points due to freezing. Optical microscopy has shown that freezing caused slight macro-structural changes on fibers, appearing grooved and cracked and an important presence of debris, probably due to formation of ice crystallites. ACCEPTED MANUSCRIPT 24 Fig. 6 a and b. Enzymatic kinetics of frozen samples. Enzymatic hydrolysis kinetics of steam explosion pretreated samples of both fiberized (up) and compacted (down) handling celluloses after freezing process. Experimental results are shown as discrete points, lines represent the theoretical model of equation 3 using the fitting parameters of Table 2. A generalized decrease in cellulose degree of hydrolysis was observed as well (Fig. 6). In this case, freezing process caused a more remarkable effect than acetone, resulting in a drastic decrease on cellulose degree of hydrolysis to values ranging from as down as 15.7% to only 27.3%. This meant an average reduction of more than 40 percentage points compared to raw cellulose fibers. Additionally, the effect of reaction time is more relevant than temperature for samples which underwent freezing. Accessibility and kinetic parameter are near identical for pairs of samples with same reaction time and handling (Table 2). The remarkable reduction in accessibility is not sufficiently counteracted by the high increase of kinetic coefficients. In these results, the degradation effect due to ice formation was clearer than it was observed for crystallinity. ACCEPTED MANUSCRIPT 25 However, it could not be possible to identify in which way or how much this process conditioned these changes. No clear relationship between the decrease of enzyme accessibility and the other properties such as crystallinity index was revealed to explain the effects of freezing. Water states and moisture could have great effects when pretreating lignocellulosic biomass (Sui & Chen, 2016) and further research should be done in this sense. 4. Conclusions The aims of this work were to perform a characterization of a commercial cellulose with two different configurations (fiberized /non-fiberized sheet), and to study the effect of steam explosion and two different preservation methods (acetone-washing and freezing). Steam explosion pretreatment was conducted at two different temperatures and reaction times (150-200 ºC, 5-30 min), and the influence of severity factor and cellulose configuration on chemical and physical characteristics was analyzed. Initial characterization of commercial celluloses returned expected values for all studied properties, with high cellulose content (91.9%) and no soluble compounds. Despite compact cellulose configuration needed three consecutives acid hydrolysis for its complete solubilization during cellulose content analysis, it showed high XG value at 48h, similar to that obtained for fiberized cellulose (~70%). Particle size measurements showed a bimodal distribution, with two peaks at 75 and 720 µm, despite a completely homogeneous water suspension for fiberized cellulose was difficult to achieve due to its entanglement and complex format. In general, steam explosion of compacted commercial cellulose seemed to be a good substitute of other mechanical treatments. No thermal degradation was observed ACCEPTED MANUSCRIPT