scieee AI-readable full text Open interactive document viewer

Analysis of degradation and evolution of model parameters of a-Si/μ-Si PV modules

Abaslioglu, Alif

Full text

1 Màster universitari en Enginyeria de l'Energia ANALYSIS OF DEGRADATION AND EVOLUTION OF MODEL PARAMETERS OF a-Si/μ-Si PV MODULES Autor: Elif ABASLIOGLU Director: Santiago SILVESTRE 2 Abstract The combination of an amorphous silicon top cell with a microcrystalline silicon bottom cell to form a stacked tandem cell, is called micromorph cell. Micromorph tandem solar cells are considered as one of the most promising new thin-film silicon solar-cell concepts. The degradation analysis of micromorph photovoltaic (PV) modules and its impact on the output power of a PV array under outdoor long term exposure located in Jaén (Spain), a relatively dry and sunny inland site with a Continental-Mediterranean climate is addressed in this study. Furthermore, solar cell model parameters extraction is presented. The parameter extraction procedure allows obtaining main model parameters of the solar cells forming the PV array from monitored data of the PV system in real operation of work. Results obtained of the evolution of each one of the solar cell model parameters along the PV system outdoor long term exposure campaign are analysed in order to achieve a better understanding of the performance changes of the PV modules and the behaviour of the output power of the PV array. Keywords: Micromorph PV modules, model parameters extraction, degradation rate. 3 Acknowledgements Firstly, I would like to express my sincere gratitude to my project director Prof. Santiago Silvestre for the continuous support of my master thesis and related research, for his patience, motivation, and immense knowledge. His guidance helped me in all the time of research and writing of this thesis. Besides my advisor, I would like to thank PhD student Sofiane Kichou for his insightful comments, encouragement and continuous help. Also I thank my friend Marc Morte and his family for their endless support during all this time. Last but not the least, I would like to thank my mother for supporting me spiritually throughout my life in general; without her support nothing would be same. 4 Table of Contents List of figures .................................................................................................................................. 5 List of tables .................................................................................................................................... 6 1. Introduction ................................................................................................................................. 7 1.1. Thin film PV modules .......................................................................................................... 7 1.2. Degradation .......................................................................................................................... 9 2. Methodology ............................................................................................................................. 11 2.1. PV Array model ................................................................................................................. 11 2.2. Output power of the PV array ............................................................................................ 12 2.3. Power – Irradiance (P-G) technique ................................................................................... 13 2.4. Parameter extraction technique .......................................................................................... 14 3. Experimental .......................................................................................................................... 19 3.1. Climate characterization of the site and PV system description ........................................ 19 4. Results and Discussions......................................................................................................... 20 4.1. Evolution of the effective peak power of the PV array ...................................................... 20 4.2. P-G Technique results ........................................................................................................ 23 4.3. Parameter extraction procedure validation ......................................................................... 30 4.4. Evolution of solar cell model parameters ........................................................................... 32 5. Conclusions ........................................................................................................................... 37 6. References ............................................................................................................................. 38 5 List of figures Figure 1. Stabilized external quantum efficiency and spectral response of micromorph solar cells ............ 8 Figure 2. Schematic structure of a tandem a-Si:H/µc-Si:H solar cell with front and back ZnO:Al contact layers grown by low-pressure CVD and with an intermediate reflector to enhance the top cell current ...... 8 Figure 3. One-diode equivalent circuit for a PV panel. [19] ....................................................................... 11 Figure 4. Effect of varying Jsco .................................................................................................................... 16 Figure 5. Effect of varying Rsh ................................................................................................................... 17 Figure 6. Effect of varying Rs ..................................................................................................................... 17 Figure 7. Effect of varying ideality factor, n .............................................................................................. 17 Figure 8. Simulink block diagram of the parameter extraction algorithm. ................................................. 18 Figure 9. The effective peak power of the PV array P*M (for G > 700 W/m2), and the monthly radiation (H) along exposure period .......................................................................................................................... 20 Figure 10. Monthly trend line outdoor stabilization process obtained with the selected data in the range of 900 W/m2 < G < 920 W/m2 and 53 ºC < T < 60 ºC ................................................................................... 22 Figure 11. Trend line outdoor stabilization process using the selected data in the range of 900 W/m2 < G < 920 W/m2 and 53 ºC < T < 60 ºC ............................................................................................................ 22 Figure 12. Stamp plot of data transition of power lines, 2011 .................................................................... 23 Figure 13. Stamp plot of data transition of power lines, 2012 .................................................................... 24 Figure 14. Stamp plot of data transition of power lines, 2013 .................................................................... 25 Figure 15. Stamp plot of data transition of power lines, 2014 .................................................................... 26 Figure 16. Monthly data transition of powerlines based gradient LCA ...................................................... 29 Figure 17. Monthly data transition of powerlines based gradient LCA, after the stabilization period ....... 29 Figure 18. Monitored and simulated DC output current obtained by using the set of parameters estimated by the extraction parameter algorithm ........................................................................................................ 30 Figure 19. Monitored and simulated DC output voltage obtained by using the set of parameters estimated by the extraction parameter algorithm ........................................................................................................ 31 Figure 20. Monitored and simulated DC power output obtained by using the set of parameters estimated by the extraction parameter algorithm ........................................................................................................ 31 Figure 21. Evolution of Io: Average values obtained by using the parameter extraction algorithm ........... 33 Figure 22. Evolution of Isc: Average values obtained by using the parameter extraction algorithm ......... 34 Figure 23. Evolution of Rsh: Mean monthly values obtained. ..................................................................... 35 Figure 24. Evolution of Rs: Mean monthly values obtained ...................................................................... 36 Figure 25. Average values of n obtained by using the parameter extraction algorithm.............................. 36 6 List of tables Table 1. Main electrical characteristics at STC of the analyzed PV field. .................................................. 19 Table 2. Annual average values of some relevant meteorological parameters recorded in Jaén ................ 19 Table 3. Monthly empirical equations based on Linear Correlation Approach .......................................... 27 Table 4. CV(RMSE) obtained for main output electrical parameters of the PV array .................................... 32 Table 5. Parameter extraction results for the 6th of October, 2011. ........................................................... 32 7 1. Introduction 1.1. Thin film PV modules Thin-film photovoltaic (TFPV) technology has plenty of advantages such as low temperature coefficient, low quantity silicon usage as raw material, low-cost manufacturing process, high energy producers, and flexibility in product design. However, several weaknesses and challenges in TFPV technology have been discussed such as low conversion efficiency; the unique nature of the instability phenomenon called light-induced degradation (LID) and long term technological risks in the field performance in terms of durability when compared with the crystalline technology [1]. The highest efficiencies among laboratory TF-Si solar cells have been achieved with a triple junction solar cell combining a hydrogenated amorphous silicon top cell with hydrogenated microcrystalline silicon middle and bottom cells (a-Si:H / μc- Si:H / μc-Si:H), or with tandem a-Si:H / μc-Si:H (micromorph) solar cells. Tandem amorphous / microcrystalline silicon thin-film solar modules with low output voltage have gained many attentions recently. A micromorph cell is usually laser scribed into cells and the cells are series connected. In order to achieve the low output voltage, the panel needs to be additionally laser scribed into several segments and the segments are then parallel connected [2]. The industrial relevance of micromorph solar cells improves enormously if they are combined with thin a-Si:H top cells, forming a 2- cell tandem stack in which the a-Si:H cell faces the sun. Given the large difference in the bandgap values of these two semiconductors (about 1.0 eV and 1.7 eV), a much better utilization of the solar spectrum and hence a higher PV efficiency is achieved. Importantly, because of the low short-circuit current density (Jsc) of stable a-Si:H cells (~13 mA/cm2), the thickness of the μc-Si:H cell in the stack does not have to be increased significantly compared to a stand-alone μc-Si:H cell. Besides, micromorph solar cells tend to have open circuit voltage around 0.54 V [3] [4]. As it can be seen clearly in Figure 1, the micromorph tandem cells offer a wider range of the sun spectrum. 8 Figure 1. Stabilized external quantum efficiency and spectral response of micromorph solar cells [5] [6] A schematic view of a micromorph solar cell is shown in Figure 2. In the multi-junction amorphous/microcrystalline Si solar cells, the top a-Si:H absorber layer is made as thin as possible (typically 0.2-0.3 µm) to minimize the light-induced efficiency degradation. Figure 2. Schematic structure of a tandem a-Si:H/µc-Si:H solar cell with front and back ZnO:Al contact layers grown by low-pressure CVD and with an intermediate reflector to enhance the top cell current [6] The intermediate reflector (IR) placed between the a-Si:H and µc-Si:H cells reflects the light back into the top cell and thus allows reduction of the thickness of the a-Si:H absorber layer without compromising the short-circuit current of the top cell, which sets 9 the current through the entire tandem device. Additionally, the IR improves current matching in tandem cells by reducing the short-circuit current of the bottom cell, which is typically excessive and thus partially wasted. The IR is made of a material with a lower refractive index (n ~ 1.5 - 2.2) compared to the a-Si:H (n ~ 4) and µc-Si:H absorbers (n ~ 3.4). The IR layer obviously should be as conductive as possible in order to minimize electrical losses. ZnO was initially used as a material for the intermediate reflectors. Moreover, scattering of blue-green light absorbing in the top cell can be further enhanced by roughening of the IR top surface with a typical feature size of around 300 nm, while keeping soft or U shape morphology with feature size of 1 µm for the bottom µc-Si:H cell. This approach has been termed as asymmetric IR in the literature. [6] 1.2. Degradation Due to the disordered nature of amorphous silicon, a-Si solar cells are subject to the Staebler-Wronski effect, which reduces the solar cell efficiency by up to 15 percent within the first months of exposure. [2] [7] [8] [9] [10] Even though the stable µc-Si:H bottom cell contributes to a better stability of the entire micromorph tandem cell under light-soaking, micromorph cells show light-induced degradation (LID) too. In fact, it could be shown that the LID of the micromorph cell is due to the amorphous cell alone. Despite the fact that the concept of a micromorph solar cell brings progress via a new stable bottom cell into the thin-film silicon scenario, the stability of the amorphous silicon top cell remains still the crucial topic [11]. This undesired effect is triggered by recombination. The released recombination energy induces defects in the amorphous network - which is why this effect is not observed in crystalline wafer solar cells. This effect gradually tends to stabilize at power rates ranging from 10% to 30 % of the nominal power of the PV module. However, thermal annealing of the a-Si for several hours at 150°C reverses these effects [8]. This degradation affects especially the internal parameters of the solar cell as the short circuit current, ideality factor, saturation current and series and shunt resistances [12] [13]. The degradation rate can be based on the comparison of the monitoring outdoor 16 Eq. (7) can also be written, substituting Ioref as a function of the short-circuit current: Isc and open circuit voltage: Voc of the solar cell, as follows: 𝐼𝑜= 𝐼𝑠𝑐 𝑒(𝐸𝑔𝑜 𝑉𝑡𝑜−𝐸𝑔 𝑉𝑡) 𝑒(𝑉𝑜𝑐 𝑛 𝑉𝑡𝑜)−1 (𝑇𝑐 𝑇𝑐∗)3 (16) The value of the energy bandgap of the semiconductor at any cell temperature Tc is given by: 𝐸𝑔=𝐸𝑔𝑜−𝛼𝑔𝑎𝑝 𝑇𝑐2 𝛽𝑔𝑎𝑝+𝑇𝑐 (17) where gap and gap are fitting parameters characteristic of the semiconductor. In order to see how these parameters affect the module performance, current – voltage and power – voltage curves are plotted by using different values of mentioned parameters. It is observed that when Jsco increases, short circuit current of the cell increases too. When series resistance Rs increases, power output of the cell decreases significantly. On the other hand, varying Rsh and ideality factor has less effect on the cell’s performance; that just makes a small change in fill factor. In the following figures, the effect of varying these parameters can be seen. Figure 4. Effect of varying Jsco 17 Figure 5. Effect of varying Rsh Figure 6. Effect of varying Rs Figure 7. Effect of varying ideality factor, n 18 The parameter extraction algorithm evaluates: Iph, Rs, Rsh, Io and n by using Eqs. (4) – (9). Daily profiles of monitored electrical parameters –namely, current and voltage at the DC output of the PV array, together with G and Tc - are used as inputs of the parameter extraction algorithm. A nonlinear regression algorithm based on the Levenberg–Marquardt method was applied to both data sets: The daily monitored data from the PV array in real conditions of work and simulation results generated by using the described model, in order to minimize the following quadratic function [31] [32]:   2 1 ),()(  ViIIiSN i    (18) where  =f(Iph,Io,Rs,Rsh,n). The designed toolbox in Simulink used for parameter extraction process is illustrated in the following figure. Figure 8. Simulink block diagram of the parameter extraction algorithm. The result of the parameter extraction algorithm is a set of solar cell model parameters that allow the best approach to the daily evolution of output current and voltage of the PV array. 19 3. Experimental 3.1. Climate characterization of the site and PV system description The PV system is formed by 8 micromorph PV modules and installed outdoors on the flat roof of the High Technical School building in University of Jaén (Latitude: 37º 47' 14.35'' N, Longitude: 3º 46' 39.73'' W, Altitude: 511 m). The system is connected to the grid by using a SMA Sunny Boy model SB1200 inverter [33]. The SMA Sunny SensorBox device was also installed in the same platform in order to measure solar radiation, module and ambient temperatures together with wind speed. The temperature sensor provided by SMA to be used with the Sunny SensorBox was pasted to the rear surface of the modules under test. An additional irradiance sensor (a pyranometer) was also installed. The period under exposure ranges from late July 2011 to mid-December 2014. Onsite measurements of DC voltage and current are recorded at the inverter input. Data were taken at 5-minute intervals. More detailed information about the PV system is given in the following table. Table 1. Main electrical characteristics at STC of the analyzed PV field. (Values derived from the PV module manufacturers' data sheet) Module Techn. Configuration (Ns x Np) Maximum Power (Wp) Open Circuit Voltage (V) Short Circuit Current (A) Voltage at MPP (V) Current at MPP (A) a-Si/µc-Si 2 x 4 880 284 5 216 4.08 Jaén is a dry and sunny inland site, with a Continental-Mediterranean climate. Table 2 summarizes the characteristics of the field climate. Table 2. Annual average values of some relevant meteorological parameters recorded in Jaén Horizontal irradiation (kWh/m2) Ambient temperature (ºC) Min. ambient temperature (ºC) Max. ambient temperature (ºC) Relative humidity (%) Rainfall (mm) Barometric pressure (hPa) 2038 16.9 11.4 22.4 63 558 954.1 20 3. Results and Discussions 4.1. Evolution of the effective peak power of the PV array For the analysis of the evaluation of the effective peak power of the array, P*M, and the monthly radiation, H, along the exposure time is plotted. The graph can be seen in the following figure. Figure 9. The effective peak power of the PV array P*M (for G > 700 W/m2), and the monthly radiation (H) along exposure period As it is seen in the graphic above, in the first months of exposure a decrease of P*M is observed due to the LID phenomenon. The decrease occurs more slightly compared to a-Si solar cells because of the µc-Si layer. Also, a seasonal variation of P*M can be seen clearly. This seasonality in PV modules has been reported in various studies of the literature [7] [5]. The initial decrease in output power of the array is followed by an increase over the summer months, a decrease over winter months and once again an increase over summer months. The regeneration on summer months can be attributed to spectral effects [34], thermal regeneration [8] [35] and light-induced annealing [14]. y = -1,5006x + 816,14 0 50 100 150 200 250 300 350 400 0 100 200 300 400 500 600 700 800 900 1000 H (kWh/m².month) Effective Power (W) Time (month) P*M at G>700 kW/m2 [W] H mensual value [kWh/m².month] Linear (P*M at G>700 kW/m2 [W]) 21 The degradation rate, RD, can be analysed by a linear least square fitting method. This method is applied to the monthly effective peak power of the PV array, P*M, calculated by using Eq. 19 and monitored data. The degradation per year can be calculated by linear regression (LR) by using the trend line equation: 𝑦=𝑚𝑥+𝑐 (19) where m is the slope of line and c is the y intercept. Thereby, the degradation rate per year RD (%) can be calculated as follows [36]: 𝑅𝐷=10012𝑚 𝑐 (20) The degradation rate calculated from the trend line is -2.20638 ± 0.15 %/year. The analytical uncertainty reported along with the degradation rate was determined from the standard errors of the linear fit. The amount of LID phenomenon depends on the thickness of a-Si layer, the distribution of light, spectrum, and temperature at the specific location of the PV array. In order to analyse the stabilization period of the PV array, a second monitoring data filtering process was carried out by following the procedure used in previous reported studies [7]. One point for each month of the monitored data for the tilted irradiance and working PV module temperature in the range of 900 W/m2 < G < 920 W/m2 and 53 ºC < T < 60 ºC was selected. From the data obtained in the filtering process; array DC power, irradiance and cell temperature data for the first 20 months of exposure are plotted in Figure 10. The stabilization period was observed to start after 5 months of operation in Jaen. The trend line is obtained by sixth polynomial correlation with R2 equal to 0.9499. As it can be seen clearly, the result shows a rapid decrease after exposure to natural sunlight due to LID phenomenon. 22 Figure 10. Monthly trend line outdoor stabilization process obtained with the selected data in the range of 900 W/m2 < G < 920 W/m2 and 53 ºC < T < 60 ºC Figure 11. Trend line outdoor stabilization process using the selected data in the range of 900 W/m2 < G < 920 W/m2 and 53 ºC < T < 60 ºC y = 5E-13x6-1E-07x5+ 0,0137x4- 747,82x3+ 2E+07x2- 4E+11x + 3E+15 R² = 0,9499 0 10 20 30 40 50 60 70 500 550 600 650 700 750 800 850 900 950 Cell Teperature (°C) Array DC power (W), Irradiance (W/m²) Exposure Time (Month) G [W/m²] Pdc [W] Tc [°C] Poly. (Pdc [W]) y = -0,0065x + 901,89 0 10 20 30 40 50 60 70 500 550 600 650 700 750 800 850 900 950 Cell Teperature (°C) Array DC power (W), Irradiance (W/m²) Exposure Time (Month) G [W/m²] Pdc [W] Tc [°C] Linear (Pdc [W]) 23 Figure 11 shows the set of data after the first 15 months of operation and the trend line for the DC output power of the array obtained by linear correlation. The stabilized level of DC output power of the array is around 640 W in the range of G and Tc considered in data filtering process. Power line demonstrates almost a constant trend after the stabilization period. Concurrently with the linear trend of the power line, a sinusoidal form attributable to the seasonal effects can also be observed. The effect of seasonal oscillation remains after the stabilization period for about 5 % variation from the stabilized level of DC power. 4.2. P-G Technique results As mentioned before, in this proposed technique, two main indicators are provided as a boundary condition, PDC_initial_predict (red) and PDC_stabilized_predict (green). The measured DC array power is plotted in blue and it is expected to change the tendency from the initial values to the stabilized ones in the course of time. The monthly variations are presented as a stamp plot for each month and the extracted datasets through the proposed P–G technique are introduced as illustrated in the following figures. Figure 12. Stamp plot of data transition of power lines, 2011 24 Figure 13. Stamp plot of data transition of power lines, 2012 25 Figure 14. Stamp plot of data transition of power lines, 2013 32 The coefficient of variation of the root mean square errors, CV(RMSE) between both data sets (real measured data and simulation results) are calculated by using the following formula: 𝐶𝑉(𝑅𝑀𝑆𝐸) =√∑(𝑥𝑖 −𝑥𝑖 )2 𝑁 𝑖=1 𝑁 𝑥 (21) where 𝑥𝑖 is the real measured data, 𝑥𝑖  is simulation results, N is the number of data points, 𝑥 is the mean of real measured values. CV(RMSE) results and extracted parameters for one sample day are given in the following tables. Table 4. CV(RMSE) obtained for main output electrical parameters of the PV array RMSCurrent [%] RMSVoltage [%] RMSPower [%] 1.29 2.44 2.60 Table 5. Parameter extraction results for the 6th of October, 2011. Day Io [A] Jsco [A] Rsh [Ω] Rs [Ω] n 10/6/2011 9.15 x 10-8 0.021461 9.6602 0.045587 1.2642 4.4. Evolution of solar cell model parameters As it was mentioned in the methodology part, the monthly average value of each one of the model parameters was calculated for the whole monitoring campaign included in this study. The seasonal variation of micromorph PV modules behaviour is also observed in the evolution of the solar cell model parameters. The variation obtained for the saturation current, Io, is shown in Figure 21. Eq. (16) gives the variation of the band-gap as a function of temperature. The higher temperatures in summer period decrease the band-gap resulting in a decrease in open- 33 circuit voltage [16]. Temperature has also a strong effect on the variation of the saturation current as shown in Eq. (16). The combination of band-gap reduction and strong increase of temperature in summer periods along with the increase in short circuit current due to LID effect lead to an increase of the saturation current despite the reduction of recombination effects in summer. However, the combination of recombination and band-gap reductions results just in a variation of less than one order of magnitude in the saturation current between summer and winter periods. Figure 21. Evolution of Io: Average values obtained by using the parameter extraction algorithm Another extracted solar cell parameter, short circuit current, Isc, also shows a continuous decrease throughout the exposure time. (See Figure 22) After the first 5 months, it shows a more stable trend. However, a seasonal effect on Isc can also be seen clearly in Fig. 22, being the predominant factor that contributes a large improvement to output power during summer time. There is an important decrease in AM from winter to summer and a favourable spectral distribution of the solar irradiance during summer especially in the ultraviolet region. The improvement in output current during summer time is due to the effect of solar spectral irradiance and to thermal-recovery of the LID [16] [34]. The lower temperatures in winter also reduce the thermal recovery rate for the 0,00E+00 2,00E-08 4,00E-08 6,00E-08 8,00E-08 1,00E-07 1,20E-07 1,40E-07 1,60E-07 1,80E-07 2,00E-07 Io (A) Exposure Time (month) 34 a-Si solar cells. The minimum value of Isc in the worst winter months is approximately 12% less than the peak value of this parameter in the months of August. This reduction is smaller compared to a-Si results shown in the literature [37]. Figure 22. Evolution of Isc: Average values obtained by using the parameter extraction algorithm Figure 23 shows the evolution of the mean monthly value obtained by the parameter extraction algorithm for the shunt resistance, Rsh, along the monitoring campaign. For the first 5 months, there is a 57% of decrease. After the stabilization period, shunt resistance continues to decrease but with a lower rate, 22%. As a final result, it is observed that Rsh reduces to 30% of its initial value. The reduction of Rsh in TF solar cells under outdoor exposure for long periods of time has been previously studied ın the literature [12] [16]. Additionally, the evolution of Rsh shows the same seasonal trend that the evolution of the output power of the PV array and Isc as expected. 1,85 1,9 1,95 2 2,05 2,1 2,15 2,2 2,25 2,3 2,35 Isc (A) Exposure Time (month) 35 Figure 23. Evolution of Rsh: Mean monthly values obtained. The series resistance, Rs, shows a continuing increase along the monitoring campaign. The values of Rs go from an initial value of 0,03  to a final value of 0,06 . The seasonal effect can be also observed in the trend of Rs that presents higher values in winter, with maximum values in the month of December, and reduced values in summer, with minimum values in the month of August. The behaviour of Rs shown in Figure 24 is in accordance with precious works reported in the literature for TF solar cells [12] [16]. Moreover, the reduction of Isc observed in winter is partially due to the increase of Rs. Eq. 1 can be particularized in short circuit conditions, V = 0, and rewritten as follows: Rsh IscRs IphIsc  (22) As can be seen in Eq. 22, the combination of higher values of Rs and lower values of Rsh in winter periods results in a decrease of Isc. The effect is the opposite in summer periods, where Rsh presents higher values while Rs and Isc decrease. 0 1 2 3 4 5 6 7 8 9 10 11 Rsh (Ω) Exposure Time (month) 36 Figure 24. Evolution of Rs: Mean monthly values obtained Figure 25 illustrates the evolution of the ideality factor n, obtained by the parameter extraction technique. It can be seen that the evolution of the ideality factor for this kind of solar cell shows seasonality like as the other extracted parameters. The evolution of n is opposite to the trend shown by the saturation current, as expected. The ideality factor shows a small reduction in summer while it increases in winter periods. However, the value of n fluctuates around a mean value of n = 1.2 and the seasonal variations are small. This fact indicates that the diode included in the equivalent circuit of the solar cell corresponding to the five parameter model is dominated by the μc-Si:H substrate (bottom cell). Figure 25. Average values of n obtained by using the parameter extraction algorithm 0 0,01 0,02 0,03 0,04 0,05 0,06 0,07 Rs(Ω) Exposure Time (month) 1,1 1,12 1,14 1,16 1,18 1,2 1,22 1,24 1,26 1,28 Ideality factor - n Exposure Time (month) 37 5. Conclusions The degradation modes of micromorph PV modules and how they affect the performance of PV modules in a relatively dry and sunny inland site with a Continental- Mediterranean climate is analyzed in this study. The data used in this study was obtained under outdoor long term exposure of the PV system in Jaén from late July 2011 to mid-December 2014. A reduction of the DC power of the PV array by about 12.3% was observed in the first month of outdoor deployment. The stabilization period was observed to start after 5 months of operation with a decline of the DC power by the relative percentage of 15.9 % and then it is stabilized. However, the effect of seasonal oscillation remains after the stabilization period for about 5 % variation from the stabilized level of DC power. Solar cell parameters identification is also addressed in this study by using a parameter extraction technique. The sets of solar cell model parameters obtained by using the parameter extraction technique are able to reproduce the behavior of the PV array in real conditions of work with a good accuracy degree. The parameter extraction technique is able to evaluate the temporal evolution of main solar cell model parameters and helps to understand the evolution of the entire system at PV module level. The seasonal variation of micromorph PV modules behaviour was also observed in the evolution of the solar cell model parameters. The evolution of each one of the model parameters along the outdoor long term exposure of the PV system has been analyzed and allows achieving a better understanding of the performance changes of the PV modules and the evolution of the output power of the PV array. 38 6. References [1] A. Čampa, M.Meier, M.Boccard, L.V.Mercaldo, M.Ghosh, C.Zhang, T.Merdzhanova, J.Krč, F.- J.Haug and M.Topič, "Micromorph silicon solar cell optical performance: Influence of intermediate reflector and front electrode surface texture," Solar Energy Materials & Solar Cells, vol. 130, pp. 401-409, 2014. [2] C.-Y. Tsai and C.-Y. Tsai, "Development of Amorphous/Microcrystalline Silicon Tandem Thin-Film Solar Modules with Low Output Voltage, High Energy Yield, Low Light-Induced Degradation, and High Damp-Heat Reliability," Journal of Nanomaterials, Hindawi Publishing Corporation, vol. 2014, no. Article ID 86174, p. 10, 2014. [3] S. Pizzini, Advanced Silicon Materials for Photovoltaic Applications, John Wiley & Sons, Ltd., 2012. [4] H. Keppner, J. Meier, P. Torres, D. Fischer and A. Shah, "Microcrystalline silicon and micromorph tandem solar cells," Applied Physics A Materials Science & Processing, vol. 69, p. 169–177, 1999. [5] J. Sutterlueti, R. Kravets, M. Keller, H. Knauss, I. Sinicco and A. Huegli, "Energy Yield Optimiziation and Seasonal Behaviour of Micromorph® Thin Film Modules," in 25th European Photovoltaic Solar Energy Conference and Exhibition / 5th World Conference on Photovoltaic Energy Conversion, Valencia, Spain, 6-10 September 2010. [6] V. AVRUTIN, N. IZYUMSKAYA and H. MORKOC, "Amorphous and micromorph Si solar cells: current status and outlook," Turkish Journal of Physics, TÜBİTAK, vol. 38, no. fiz-1406-14, pp. 526- 542, 2014. [7] M. Hussin, S. Shaari, A. Omar and Z. Zain, "Amorphous silicon thin-film: Behaviour of lightinduced degradation," Renewable ans Sustainable Energy Reviews, no. 43, pp. 388-402, 2015. [8] Y. Yamawaki, S. Mizukami, A. Yamazaki and H. Takahashi, "Thermal recovery effect on lightinduced degradation of amorphous silicon solar module under the sunlight.," Sol. Energy Mater. Sol. Cells, vol. 47, no. doi:10.1016/S0927-0248(97)00033-0, pp. 125-134, 1997. [9] D. L. Staebler and C. R. Wronski, "Reversible conductivity changes in discharge‐produced amorphous Si," Applied Physics Letters, vol. 31(4), pp. 292-294, 1977. [10] S. Spataru, P. Hacke, D. Sera, C. Packard, T. Kerekes and R. Teodorescu, "Temperature-dependency analysis and correction methods of in situ power-loss estimation for crystalline silicon modules undergoing potential-induced degradation stress testing," Prog. Photovolt. Res. App., 2015. [11] A. V. Shah, H. Schade, M. Vanecek, J. Meier, E. Vallat-Sauvain, N.Wyrsch1, U. Kroll, C. Droz and J. Bailat, "Thin-film Silicon Solar Cell Technology," PROGRESS IN PHOTOVOLTAICS: RESEARCH AND APPLICATIONS, vol. 12, no. Special Issue (DOI: 10.1002/pip.533), pp. 113-142, 2004. [12] E. Van Dyk and E. Meyer, "Analysis of the effect of parasitic resistances on the performance of 39 photovoltaic modules.," Renewable Energy, vol. 29, pp. 333-344, 2004. [13] S. Voswinckel, V. Wesselak and B. Lustermann, "Behaviour of amorphous silicon solar modules: A parameter study.," Solar Energy , vol. 92, p. 206–213, 2013. [14] E. Van Dyk, a. Audouard, E. Meyer and C. Woolard, "Investigation of the degradation of a thin-film hydrogenated amorphous silicon photovoltaic module.," Sol. Energy Mater. Sol. Cells , no. 91, p. 167–173, 2007. [15] G. Kleiss, K. Bucher, P. Ragot and M. Chantant, "Monitoring outdoor performance and photodegradation of a-Si:H modules by evaluation of continuously measured I-V curves.," in Proc. 1994 IEEE 1st World Conf. , 1994. [16] C. Radue and E. van Dyk, "A comparison of degradation in three amorphous silicon PV module technologies.," Sol. Energy Mater. Sol. Cells, vol. 94, p. 617–622, 2010. [17] A. Phinikarides, G. Makrides and G. Georghiou, "Comparison of analysis methodes for the calculation of degradation rates of different photovoltaic thechnologies," in Proceedings of the 28th European photovoltaic solar energy conference and exhibition, 2013. [18] A. Phinikarides, N. Kindyni, G. Makrides and G. Georghiou, "Review of photovoltaic degradation rate methodologies.," Renew. Sustain. Energy Rev. , vol. 40, p. 143–152, 2014. [19] L. Castañer and S. Silvestre, Modelling Photovoltaic Systems using Pspice, Wiley, 2002. [20] M. Di Vincenzo and D. Infield, "Detailed PV array model for non-uniform irradiance and its validation against experimental data.," Sol. Energy , vol. 97, p. 314–331, 2013. [21] A. Chouder, S. Silvestre, N. Sadaoui and L. Rahmani, "Modeling and simulation of a grid connected PV system based on the evaluation of main PV module parameters.," Simul. Model. Pract. Theory , vol. 20, p. 46–58, 2012. [22] A. Chouder and S. Silvestre, "Automatic supervision and fault detection of PV systems based on power losses analysis," Energy Convers. Manag., vol. 51, p. 1929–1937, 2010. [23] H. Tsai, "Insolation-oriented model of photovoltaic module using Matlab/Simulink," Sol. Energy , vol. 84, p. 1318–1326, 2010. [24] M. AlHajri, K. El-Naggar, M. AlRashidi and a. K. Al-Othman, "Optimal extraction of solar cell parameters using pattern search," Renew. Energy , vol. 44, p. 238–245, 2012. [25] A. Chouder, S. Silvestre, B. Taghezouit and E. Karatepe, "Monitoring, modelling and simulation of PV systems using LabVIEW.," Sol. Energy, vol. 91, p. 337–349, 2013. [26] F. Martínez-Moreno, E. Lorenzo, J. Muñoz and R. Moretón, "On the testing of large PV arrays.," Prog. Photovoltaics Res. Appl., vol. 20, p. 100–105, 2012. [27] J. Muñoz, E. Lorenzo, M. Carrillo J. and R. Moretón, "Design of a twin capacitive load and its application to the outdoor rating of photovoltaic modules," Prog. Photovolt: Res. Appl., vol. 23, p. 40 247–252, 2015. [28] F. Martínez-Moreno, E. Lorenzo, J. Muñoz and R. Moretón, "On the testing of large PV arrays.," Prog. Photovoltaics Res. Appl. , vol. 20, p. 100–105, 2012. [29] G. Nofuentes, B. García-Domingo, J. V. Muñoz and F. Chenlo, "Analysis of the dependence of the spectral factor of some PV technologies on the solar spectrum distribution.," Appl. Energy, vol. 113, p. 302–309, 2014. [30] CIEMAT, "Informe de medida de módulos fotovoltaicos," PVLabDER/ITC006_M, Madrid, 2011. [31] A. Chouder and S. Silvestre, "Analysis Model of Mismatch Power Losses in PV Systems.," Sol. Energy Eng. , vol. 131, no. doi:10.1115/1.3097275, 2009. [32] W. Durisch and J.-C. Mayor, "Application of a generalized current/voltage model for solar cells to outdoor measurements on a SIEMEN SM 110-module.," in 3rd World Conf. onPhotovoltaic Energy Conversion, 2003. [33] F. Fabero, M. Torres-Ramírez and G. Nofuentes, "TECHNICAL REPORT: FIELD TEST OF KANEKA PV MODULES (models G-EA060 and U-EA110) IN JAÉN," CIEMAT, UJAEN, 2013. [34] D. Carlson, "Monolithic amorphous silicon alloy solar modules.," Sol. Energy Mater. Sol. Cells, vol. 78, no. doi:10.1016/S0927-0248(02)00455-5, p. 627–645, 2003. [35] R. Ruther, J. Del Cueto, G. Tamizh-Mani, A. Montenegro, S. Rummel, A. Anderberg and B. Von Roedern, "Performance test of amorphous silicon modules in different climates - Year four: Progress in understanding exposure history stabilization effects," in Conf. Rec. IEEE Photovoltaic Spec., 2008. [36] V. Sharma, O. Sastry, A. Kumar, B. Bora and S. Chandel, "Degradation analysis of a-Si, (HIT) hetro-junction intrinsic thin layer silicon and m-C-Si solar photovoltaic technologies under outdoor conditions.," Energy, vol. 72, no. doi:10.1016/j.energy.2014.05.078, p. 536–546, 2014. [37] S. Kichou, S. Silvestre, G. Nofuentes, M. Torres-Ramírez, A. Chouder and D. Guasch, "Characterization of degradation and evaluation of model parameters of amorphous silicon photovoltaic modules under outdoor long term exposure," Energy, vol. In press, 2016. [38] D. Fischer, S. Dubail, J. A. A. Selvan, N. P. Vaucher, R. Platz, C. Hof, U. Kroll, J. Meier, P. Torres, H. Keppner, N. Wyrsch, M. Goetz, A. Shah and K.-D.Ufert, "THE "MICROMORPH" SOLAR CELL: EXTENDING A-SI:H TECHNOLOGY TOWARDS THIN FILM CRYSTALLINE SILICON," in 1nd World Conf. Photovolt. Energy Conf. p. 409, Hawaii, 1994. [39] N. Aoun, R. Chenni, B. Nahman and K. Bouchouicha, "Evaluation and Validation of Equivalent Five-Parameter Model Performance for Photovoltaic Panels Using Only Reference Data," Energy and Power Engineering, vol. 6, pp. 235-245, 2014.