scieee AI-readable full text Open interactive document viewer

The need to consider flexural post-cracking creep behavior of macro-synthetic fiber reinforced concrete

Pujadas Álvarez, Pablo,Blanco Álvarez, Ana,Pialarissi Cavalaro, Sergio Henrique,Fuente Antequera, Albert de la,Aguado de Cea, Antonio

Abstract

The flexural creep of plastic fiber reinforced concrete (PFRC) is a controversial issue since significant doubts regarding the suitability of this type of fiber and its influence in the long-term behavior of the material still exist. The objective of this paper is to evaluate the post-cracking creep response of PFRC beams under flexural load in comparison with that of steel fiber reinforced concrete (SFRC) beams. The aim is to explore how the pre-crack opening and the environmental condition affect the long term behavior of each material and identify differences. An experimental program was conducted with 30 concrete beams with dimension of 150 × 150 × 600 mm reinforced with plastic or steel fibers subjected to a 4-point bending creep test for 5 months under 2 environmental conditions. Results showed that the flexural creep coefficient of PFRC is 2 times bigger than that of SFRC. Despite that, the use of plastic fibers as reinforcement should not be rejected as long as the additional creep is considered in the design and the crack widths are limited to reduce the risk of tertiary creep.

Full text

THE NEED TO CONSIDER FLEXURAL POST-CRACKING CREEP BEHAVIOR OF MACRO-SYNTHETIC FIBER REINFORCED CONCRETE P. Pujadas, A. Blanco, S. Cavalaro, A. de la Fuente, A. Aguadoa The flexural creep of plastic fiber reinforced concrete (PFRC) is a controversial issue since significant doubts regarding the suitability of this type of fiber and its influence in the long-term behavior of the material still exist. The objective of this paper is to evaluate the post-cracking creep response of PFRC beams under flexural load in comparison with that of steel fiber reinforced concrete (SFRC) beams. The aim is to explore how the precrack opening and the environmental condition affect the long term behavior of each material and identify differences. An experimental program was conducted with 30 concrete beams with dimension of 150x150x600 mm reinforced with plastic or steel fibers subjected to a 4-point bending creep test for 5 months under 2 environmental conditions. Results showed that the flexural creep coefficient of PFRC is 2 times bigger than that of SFRC. Despite that, the use of plastic fibers as reinforcement should not be rejected as long as the additional creep is considered in the design and the crack widths are limited to reduce the risk of tertiary creep. Keywords: plastic fiber - synthetic fiber - FRC - four-point bending test - creep THE NEED TO CONSIDER FLEXURAL POST-CRACKING CREEP BEHAVIOR OF MACRO-SYNTHETIC FIBER REINFORCED CONCRETE P. Pujadasa, A. Blancoa, S. Cavalaroa, A. de la Fuentea, A. Aguadoa a Department of Civil and Environmental Engineering, Division of Geotechnical Engineering and Geosciences, School of Civil Engineering, Universitat Politècnica de Catalunya (UPC-Barcelona Tech), Jordi Girona 1-3, Building D2, Barcelona, Spain. 1-Introduction Fiber-reinforced concrete (FRC) is a competitive material for structural applications that demand a combination of moderate post-cracking tensile bearing capacity and high toughness [1–5]. Studies have shown that it is possible to achieve the desired structural performance by substituting either partial [6–9] or completely [10] the traditional reinforcement by fibers. Over the past decade, due to the heightened interest of the scientific community in macro-synthetic fibers [11], significant effort has gone into the development of new types of plastic fibers for structural applications [4, 12]. In this area, [13–15] demonstrated the feasibility of plastic fibers as the sole reinforcement (without rebars) in slabs under hyperstatic configurations, [16] showed that these fibers could be used as shear reinforcement in both wide-shallow and deep beams, and [17] experimentally tested their use as a reinforcement against localized splitting of precast tunnel segments. Despite the advances in the field of concrete reinforced with plastic fibers, the use of steel fibers still predominates in elements with high structural responsibility. One of the most recurrent reasons for that choice is the uncertainty regarding the long-term performance of plastic-fiber reinforced concrete (PFRC). Under sustained load, concrete deformation gradually increases with time and may eventually be many times bigger than the initial value. This phenomenon – also known as creep – could affect negatively the structural performance of the elements in service. In certain situations, it may impair the serviceability of the structure and even lead to failure at a lower load than the static ultimate load [18–20]. From a design-oriented perspective, creep deformations should also be taken into account in the medium-to-long-term behavior of FRC [21, 22]. According to [18] and [20], creep of cracked FRC elements subjected to bending is the result of 3 components: concrete creep under compression, time-dependent debonding behavior at the fiber-matrix interface and fiber creep at a material level under tensile stress. In the case of Steel Fiber-Reinforced Concrete (SFRC), the creep deformation of the fibers is considered small so that the total creep is governed by the slow debond and pull-out of the fibers from the matrix [23, 24]. Conversely, in PFRC elements, the creep of the fiber may not be disregarded. This is a complex phenomenon that depends on the stress level, on intrinsic material properties (crystallinity and molecular orientation of the polymer) and on other external parameters (UV radiation, temperature and humidity) [25, 26]. Despite the relevance of the issue, information on flexural creep of PFRC is still limited [25], not being sufficiently addressed in design recommendations [22]. The objective of this paper is to evaluate the post-cracking creep response of PFRC beams under flexural load in comparison with that of SFRC beams. The aim is to explore how the initial crack opening and the environmental condition may affect the long term behavior of each material and to identify differences. For that purpose, an experimental program was conducted using 30 beams reinforced with either plastic or steel fibers. These beams were pre-cracked at 3 crack openings and underwent 4-point bending creep test for 5 months under 2 different environmental conditions. The results obtained highlight differences in the behavior depending on the type of fiber, and contribute to enlarge the database available in the literature regarding the flexural creep of PFRC. Moreover, the conclusions derived from this study put forward the importance of limiting in the design the maximum crack width in order to reduce the risk of unacceptable deflections and failure of PFRC elements. 2-Review of previous works Among the few studies about the uni-axial tensile creep of cracked FRC are those reported by [19] on steel fibers, by [18] and [27] on micro-synthetic fibers and by [22] on macrosynthetic fibers. Information on flexural creep behavior of FRC cracked sections in specimens [21, 28, 29] and in full-scale elements [30–32] is also available in the technical literature. More recently, [24] studied the creep behavior of pre-cracked (widths ranging from 0.2 to 3.5 mm) beams reinforced with steel fibers under a four-point bending configuration. The authors reported stable responses over 18 months for small pre-crack openings of up to 0.5 mm, regardless of the load levels. However, for pre-crack openings larger than 0.5 mm and load ratios of 0.96, relatively high crack-opening rates were observed, pointing towards possible initiation of creep failure. When the load was further increased, sudden failure occurred. [33] and [34] tested 31 SFRC specimens under four-point bending in order to investigate the effects of various parameters on creep in cracked conditions. Through a multiple linear regression, the authors concluded that the load-ratio had an effect on the flexural creep response and that the extent of such effect depended on fiber slenderness and content. [23] investigated the time-dependent behavior of cracked FRC round panels reinforced with either steel or synthetic fibers (considering 2 fiber types for each of them). The author reported that post-crack creep coefficients were insensitive to load ratio for the SFRC and for one of the two PFRC tested, while the creep coefficient of the second PFRC was sensitive to the load ratio. Although studies are generally limited to a single pre-crack width, tests performed by [35], [24] and [33] had a pre-cracking range between 0.2 and 3.5 mm. These works concur that crack-width directly affects the creep phenomenon. 3-Experimental method In the present study, the time-dependent behavior under sustained load was investigated through 30 flexural 4‐point bending tests on beams (with dimensions of 150x150x600 mm) reinforced with either plastic fibers (PF) or steel fibers (SF). The tests were performed in two environmental conditions (S1 and S2) over 5 months considering different pre-crack widths (0.25 mm, 1.5 mm and 2.5 mm). 3.1-Materials and mix design All concrete mixes were prepared in a 750-liter vertical-axis mixer. First, the dried components were mixed for one minute. Subsequently, the water was added and mixed for two minutes. Then, following the addition of the superplasticizer and the steel fibers, the concrete was mixed for two additional minutes. The total mixing time was 5‐7 minutes. 4 batches of concrete specimens were produced: 2 with 5 kg/m3 of PF and 2 with 40 kg/m3 of SF. The specifications of each series of concrete mix are presented in Table 1. The amount of superplasticizer and water were slightly adjusted to assure similar workability in all batches in order to favor similar fiber distribution in all specimens. Table 1 - Composition of the FRC mixture (in kg/m3) The plastic macro-fibers (PF) used in the tests were straight strips of polyolefin with rectangular cross-sections and a continuously embossed surface texture to improve adherence. The low-carbon steel fibers (SF) had circular cross-sections and hooked ends, being gathered into bundles with water‐soluble glue. Further details about the characteristics of both fibers are presented in Table 2. Table 2 - Fiber characteristics provided by the manufacturers The following specimens were cast for each batch: 3 prismatic beams (150x150x600 mm) for the creep test, 3 prismatic beams (150x150x600 mm) for flexural strength tests according with EN 14651:2005, 3 cylindrical samples (150x300 mm) for compressive strength tests according with UNE 83507:2004, and 3 cylindrical samples (150x300 mm) to test the modulus of elasticity in accordance with UNE 83316:1996. All of them were externally vibrated over a vibrating table at 3000 rpm for approximately 10 seconds. They were removed from the molds after 24 hours of casting and moist cured under a plastic sheet for approximately one week. After that, they were transported from the ESCOFET S.A. facilities to the Luis Agulló Laboratory of Structural Technology at the Universitat Politècnica de Catalunya (Polytechnic University of Catalonia), where they were kept in a curing room at 20±2ºC and 95% of relative humidity. Table 3 shows the average compressive strength (fcm), average modulus of elasticity (Ecm), limit of proportionality (fL) and the residual flexural tensile strengths (fR1, fR2, fR3 and fR4) corresponding to CMODs of 0.05 mm, 0.50 mm, 1.50 mm, 2.50 mm and 3.50 mm, respectively. Table 3 - Characterization of the FRC at 28 days 3.2-Test procedure The specimens were subjected to two different loading phases schematized in Figure 1. Phase 1 comprised the pre-cracking of the beams until a nominal crack width, whereas Phase 2 included the creep test. Figure 1 - Diagram of the complete test procedure In Phase 1, specimens with a 25 mm notch were placed in a closed-loop servo-hydraulic press supported by 2 rollers 450 mm apart from each other. Then, they were subjected to a 4-point bending test, using crack-mouth opening displacement (CMOD) as the control signal. In addition to the clip gauge placed at the bottom of the beam, crack-opening displacement (𝑤𝑝 𝑓) was monitored by a linear variable differential transducer (LVDT) attached to the lateral side of the specimen, 12 mm above the lower surface (see Fig. 2b). Figure 2 - Pre-cracking of the beams in Phase 1 (a) and detail of the position of the LVDT at the lateral side of the beam (b) To obtain different pre-cracking openings, the process was interrupted at 𝑤𝑝 𝑓 of approximately 0.25 mm, 1.50 mm and 2.50 mm. Table 4 shows the 𝑤𝑝 𝑓 of each beam that was tested. For the pre-cracking and the creep test, specimens were supported and loaded on the two parallel sides that were in contact with the lateral sides of the mold during the casting procedure. Table 4 - Summary of loading conditions and pre-crack width The pre-cracked beams were unloaded and immediately placed in a creep frame to initiate Phase 2 (creep test). The design of the set up for the flexural creep test was based on previous work by [36], being identical to those from [24], [33] and [34]. As depicted in Fig. 3, a predefined weight is placed over a lever arm that pivots on a fulcrum and transfers the load to the beams by means of two threaded steel bars on both sides of the beams. Figure 3 - Side view of the frame for the creep test (a), creep frame before (b) and after (c) loading. Each steel frame allowed the simultaneous test of 3 beams arranged vertically one over the other in a column. A 4-point bending test configuration was used with steel rollers to transmit the load between beams of the same column (see Fig. 3). The support over the uppermost specimens acted simultaneously as the loading points on the specimens immediately below (for which the intermediate specimen in each frame was turned). The lateral LVDT used to measure the 𝑤𝑝 𝑓 during the pre-cracking stage remained alongside the beam and was used to register the crack-opening evolution during the creep test (𝑤𝑐 𝑡). The assessment of the 𝑤𝑐 𝑡 was conducted as proposed in [21] and [24] The load level (Fc) used for the creep test was a percentage ξ (between 50% and 60%, see Table 4) of the load registered in the pre‐cracking phase (Fp). The self-weight of the beams (G) was considered for the estimation of the load level, which could not be exactly identical for the beams of the same column due to the difference in pre-cracking load and the influence of the self-weight. Load cells were employed to control the load of each frame throughout the creep test. During the creep test, 15 beams were kept in a climate‐controlled room under relatively constant conditions (environment S1). The rest of the beams were kept under laboratory conditions without any control of the temperature and the humidity (environment S2). Fig. 4 shows the temperature and humidity measured during the creep tests of beams subjected to S1 and S2. Figure 4 - Humidity and temperature throughout creep tests for environment S1 (a) and S2 (b) The total duration of the long-term loading had to be chosen so that the stabilization of the time-dependent crack widths would be reached. When loading SFRC specimens at 50% of their capacity at the pre-cracking level, [24] observed a slight increase of crack width in early ages, followed by a stabilization. [37] and [38] reported stabilization after 12 weeks (84 days). On the contrary, [39] and [40] considered that the time-dependent deformations increased continuously up to failure due to fiber debonding and pull-out. Consequently, they rejected the possibility of reaching a stabilized time-dependent crackwidth. Likewise, [41] found no stabilization of the crack width after 3-months (84 days) of loading and suggested to extend the test for a longer period of time. Considering the aforementioned, in the present experimental program, the specimens were loaded at an age t0 of 40 days and the duration of the sustained load stage was extended to 151 days (5 months) and 98 days (3.5 months) for environments S1 and S2, respectively. After that, specimens were unloaded. The nomenclature used here to refer to each beam includes the environment (S1 or S2), a back slash, the type of fiber (PF or SF), an underline, the value of the nominal 𝑤𝑝 𝑓 (0.25 mm, 1.50 mm or 2.50 mm), and the reference of the specimen. For example, S1/PF_0.25P1 indicates the specimen P1 with plastic fiber, which had been pre-cracked to a nominal opening of 0.25 mm and subjected to the creep test at environment S1. In order to maximize the observations derived from this study and the comparison of both types of fibers, the number of beams tested for each combination of variables was optimized taking into account the conditions considered more representative of reality (see Table 4). With that in mind, a bigger number of specimens were test for the pre-crack opening of 0.25 mm since it is considered more representative of SLS. Therefore, for this pre-crack opening, 5 PFRC beams were tested in environment S1, 4 PFRC beams were tested in environment S2, 3 SFRC beams were tested in environment S1 and 6 SFRC beams were tested in environment S2. Consequently, a smaller number of elements were available for testing with pre-crack openings of 1.50 mm and 2.50 mm (6 PFRC and 6 SFRC, in total). 4-Experimental results and discussion 4.1-Primary and secondary creep in environment S1 Fig. 5 presents the increment of crack opening (∆𝑤𝑐 𝑡) over time for beams in the environment S1 with 𝑤𝑝 𝑓 of 0.25 mm and 1.50 mm. The ∆𝑤𝑐 𝑡 was calculated as the difference between the crack opening at a certain time and that measured at the beginning of the creep test immediately after applying the load. Figure 5 - Evolution of ∆𝑤𝑐 𝑡 over time for specimens with 𝑤𝑝 𝑓 of 0.25 mm and 1.50 mm in environment S1 After 150 days of loading, the ∆𝑤𝑐 𝑡 values registered by the specimens pre-cracked at a 𝑤𝑝 𝑓 of 0.25 mm in environment S1 varied between 0.30 and 0.45 mm for PFRC (see Fig.  The increase of crack width caused by creep was between 6 and 10 times bigger for PFRC beams in comparison with equivalent beams with SFRC. This may be the result of a more intense damage of the fiber-matrix interface for the same precrack opening in the case of PFRC. It may also be caused by the own creep of the plastic fiber at an individual level.  The creep coefficients obtained for PFRC at 90 days were between 1.5 and 3.5. At similar loading levels and for 𝑤𝑝 𝑓 smaller than 1.50 mm, cracked PFRC can be expected to present creep coefficients around twice of those found for equivalent SFRC elements. Until this age and for both types of fiber, the creep coefficient was not affected by the pre-cracking value (𝑤𝑝 𝑓). This suggests that a reference creep coefficient could be applied in the design regarded that the crack opening is limited.  For large pre-cracking widths (2.5 mm), the plastic fiber-matrix interaction was severely damaged. Although the fibers did not break in any of the cases under analysis, the increase of the crack width over the creep tests favored fiber pull out and depleted progressively the tensile strength provided by the fibers, which caused additional increases of the crack opening. This generated an accumulation effect, an acceleration of the creep rate and, ultimately, the failure of beams with PFRC, which showed tertiary creep. These observations in no way mean that plastic fibers cannot be used for the partial or total replacement of conventional reinforcement. To safely use the material, the additional creep deformation expected should be considered in the design. Moreover, it should be ensured that creep behavior beyond the stage of secondary creep will not take place during the service life. In order to meet this requirement, crack opening and load level limitations should be defined for the design of FRC structures. This is especially important for PFRC since it is more likely to present tertiary creep. For that purpose, additional studies should be conducted about the critical pre-crack opening that may lead to tertiary creep in the case of PFRC elements. Acknowledgments The authors of this paper wish to show their gratitude for the economic support received through the Research Project BIA2010-17478: Construction Processes by means of Fiber Reinforced Concretes. The authors thank the company ESCOFET S.A. for their collaboration in the development of the experimental program. The first author acknowledges the PDJ grant provided by the Departament d’Universitats, Recerca i Societat de la Informació de la Generalitat de Catalunya. References [1] M. di Prisco, G. Plizzari, and L. Vandewalle, “Fibre reinforced concrete: new design perspectives,” Mater. Struct., vol. 42, no. 9, pp. 1261–1281, Sep. 2009. [2] J. C. Walraven, “High performance fiber reinforced concrete: progress in knowledge and design codes,” Mater. Struct., vol. 42, no. 9, pp. 1247–1260, Oct. 2009. [3] P. Pujadas, A. Blanco, S. H. P. Cavalaro, A. De La Fuente, and A. Aguado, “Multidirectional double punch test to assess the post-cracking behaviour and fibre orientation of FRC,” Constr. Build. Mater., vol. 58, pp. 214–224, 2014. [4] M. G. Alberti, a. Enfedaque, J. C. Gálvez, M. F. Cánovas, and I. R. Osorio, “Polyolefin fiber-reinforced concrete enhanced with steel-hooked fibers in low proportions,” Mater. Des., vol. 60, pp. 57–65, 2014. [5] M. G. Alberti, A. Enfedaque, and J. C. Gálvez, “Comparison between polyolefin fibre reinforced vibrated conventional concrete and self-compacting concrete,” Constr. Build. Mater., vol. 85, pp. 182–194, 2015. [6] L. Vandewalle, “Cracking behaviour of concrete beams reinforced with a combination of ordinary reinforcement and steel fibers,” vol. 33, no. April, pp. 164–170, 2000. [7] P. Pujadas, A. Blanco, A. Fuente, and A. Aguado, “Cracking behavior of FRC slabs with traditional reinforcement,” Mater. Struct., vol. 45, no. 5, pp. 707–725, Oct. 2011. [8] L. Liao, A. de la Fuente, S. Cavalaro, and A. Aguado, “Design procedure and experimental study on fibre reinforced concrete segmental rings for vertical shafts,” Mater. Des., vol. 92, pp. 590–601, 2016. [9] E. V. Sarmiento, M. R. Geiker, and T. Kanstad, “Influence of fibre distribution and orientation on the flexural behaviour of beams cast from flowable hybrid polymer–steel FRC,” Constr. Build. Mater., vol. 109, pp. 166–176, 2016. [10] A. Blanco, P. Pujadas, A. de la Fuente, S. Cavalaro, and A. Aguado, “Influence of the type of Fiber on the structural response and design of FRC slabs,” J. Struct. Eng., 2016. [11] S. Yin, R. Tuladhar, F. Shi, M. Combe, T. Collister, and N. Sivakugan, “Use of macro plastic fibres in concrete: A review,” Constr. Build. Mater., vol. 93, pp. 180–188, 2015. [12] N. Buratti, C. Mazzotti, and M. Savoia, “Post-cracking behaviour of steel and macro-synthetic fibre-reinforced concretes,” Constr. Build. Mater., vol. 25, no. 5, pp. 2713–2722, 2011. [13] P. Pujadas, A. Blanco, S. Cavalaro, and A. Aguado, “Plastic fibres as the only reinforcement for flat suspended slabs: Experimental investigation and numerical simulation,” Constr. Build. Mater., vol. 57, pp. 92–104, Apr. 2014. [14] P. Pujadas, a. Blanco, S. H. P. Cavalaro, a. Aguado, S. Grünewald, K. Blom, and J. C. Walraven, “Plastic fibres as the only reinforcement for flat suspended slabs: Parametric study and design considerations,” Constr. Build. Mater., vol. 70, pp. 88–96, Nov. 2014. [15] P. Pujadas, A. Blanco, S. Cavalaro, A. de la Fuente, and A. Aguado, “Fibre distribution in macro-plastic fibre reinforced concrete slab-panels,” Constr. Build. Mater., vol. 64, pp. 496–503, Aug. 2014. [16] A. Conforti, F. Minelli, A. Tinini, and G. a. Plizzari, “Influence of polypropylene fibre reinforcement and width-to-effective depth ratio in wide-shallow beams,” Eng. Struct., vol. 88, pp. 12–21, 2015. [17] G. Tiberti, A. Conforti, and G. a. Plizzari, “Precast segments under TBM hydraulic jacks: Experimental investigation on the local splitting behavior,” Tunn. Undergr. Sp. Technol., vol. 50, pp. 438–450, 2015. [18] W. P. Boshoff, V. Mechtcherine, and G. P. a. G. van Zijl, “Characterising the time-dependant behaviour on the single fibre level of SHCC: Part 1: Mechanism of fibre pull-out creep,” Cem. Concr. Res., vol. 39, no. 9, pp. 779–786, Sep. 2009. [19] G. Zhao, M. di Prisco, and L. Vandewalle, “Experimental investigation on uniaxial tensile creep behavior of cracked steel fiber reinforced concrete Experimental investigation on uniaxial tensile creep behavior of cracked steel fiber reinforced concrete,” Mater. Struct., pp. 0–11, 2014. [20] A. Abrishambaf, J. A. O. Barros, and V. M. C. F. Cunha, “Time-dependent flexural behaviour of cracked steel fibre reinforced self-compacting concrete panels,” Cem. Concr. Res., vol. 72, pp. 21–36, 2015. [21] J.L. Granju, P. Rossi, G. Chanvillard, B. Mesureur, A. Turatsinze, H. Farhat, C. Boulay, J.J. Serrano, P. Fakhri, O. Roque, And P. Rivillon, “Delayed behaviour of cracked SFRC beams,” pp. 511–520, 2000. [22] A. J. Babafemi and W. P. Boshoff, “Tensile creep of macro-synthetic fibre reinforced concrete (MSFRC) under uni-axial tensile loading,” Cem. Concr. Compos., vol. 55, pp. 62–69, Jan. 2015. [23] E. S. Bernard, “Influence of fiber type on creep deformation of cracked fiberreinforced shotcrete panels,” ACI Mater. J., vol. 107, no. 107, pp. 474–480, 2010. [24] R. L. Zerbino and B. E. Barragán, “Long-term behavior of cracked steel fiberreinforced concrete beams under sustained loading,” ACI Mater. J., vol. 109, no. 109, pp. 215–224, 2012. [25] N. Buratti and C. Mazzotti, “Experimental tests on the effect of temperature on the long-term behaviour of macrosynthetic Fibre Reinforced Concretes,” Constr. Build. Mater., vol. 95, pp. 133–142, 2015. [26] G. Liu, X., Huang, Y., Deng, C., Wang, X., Tong, W., Liu, Y., Huang, J., Yang, Q., Liao, X. and Li, “Study on the Creep Behavior of Polypropylene Xiaolin,” Polym. Eng. Sci., vol. 49, no. 7, pp. 1375–1382, 2009. [27] W. P. Boshoff and C. J. Adendorff, “Effect of sustained tensile loading on SHCC crack widths,” Cem. Concr. Compos., vol. 37, no. 1, pp. 119–125, 2013. [28] W. Kusterle, “Viscous material behavior of solidscreep of polymer fiber reinforced concrete.” p. 5, 2009. [29] S. Kurtz and P. Balaguru, “Postcrack creep of polymeric fiber-reinforced concrete in flexure,” Cem. Concr. Res., vol. 30, no. July 1999, pp. 183–190, 2000. [30] K. H. Tan, P. Paramasivam, and K. C. Tan, “Instantaneous and long-term deflections of steel fiber reinforced concrete beams,” ACI Struct. J., vol. 91, no. 91, pp. 384–393, 1994. [31] K. H. Tan and M. K. Saha, “Ten-year study on steel fiber-reinforced concrete beams under sustained loads,” ACI Struct. J., vol. 102, no. 102, pp. 472–480, 2005. [32] K. Tan, P. Paramasivam, and K. Tan, “Creep and shrinkage deflections of RC beams with steel fibers,” J. Mater. Civ. …, vol. 6, no. 4, 1994. [33] S. E. Arango, P. Serna, J. R. Martí-Vargas, and E. García-Taengua, “A Test Method to Characterize Flexural Creep Behaviour of Pre-cracked FRC Specimens,” Exp. Mech., vol. 52, no. 8, pp. 1067–1078, Oct. 2011. [34] E. García-Taengua, S. Arango, J. R. Martí-Vargas, and P. Serna, “Flexural creep of steel fiber reinforced concrete in the cracked state,” Constr. Build. Mater., vol. 65, pp. 321–329, Aug. 2014. [35] J. MacKay and J. F. Trottier, “Post-crack creep behavior of steel and synthetic FRC under flexural loading,” in Shotcrete: More Engineering Developments, 2004, pp. 183–192. [36] T. Bast, A. Eder, F. Regensburg, and F. Bauingenieurwesen, “Untersuchungen zum Langzeitverhalten von Faserbetonen unter Biegezugbeanspruchung – ein Zwischenbericht,” no. Bild 2, pp. 32–35. [37] H. Klinkert, J. Rosenbusch, and M. Teutsch, “Long Time Behaviour and Influence of the Height of Steel Fibre Reinforced Concrete Members,” 2002. [38] R. Gettu, “Test and Design Methods for Steel Fibre Reinforced Concrete-Creep in the Post-Cracked Region,” 2002. [39] J. MacKay, “Behaviour of steel and synthetic fibre reinforced concrete under flexural creep loading.,” Dalhousie University, Halifax., 2002. [40] Jonh T. Cochrane, “Flexural Creep Behaviour of fibre Reinforced concrete under high Temperatures,” Dalhousie University, Halifax., 2003. [41] O. Bernard, F.-J. Ulm, and E. Lemarchand, “A multiscale micromechanicshydration model for the early-age elastic properties of cement-based materials,” Cem. Concr. Res., vol. 33, no. 9, pp. 1293–1309, Sep. 2003. [42] K. Kovler, “Interdependence of Creep and Shrinkage for Concrete under Tension,” J. Mater. Civ. Eng., vol. 7, no. 2, pp. 96–101, 1995. [43] Z. P. Bazant, “Drying creep of concrete:constitutive model and new experiments separating its mechanisms.,” Mater. Struct., vol. 27, pp. 3–14, 1994. [44] W. P. Boshoff, V. Mechtcherine, and G. P. a. G. van Zijl, “Characterising the time-dependant behaviour on the single fibre level of SHCC: Part 2: The rate effects on fibre pull-out tests,” Cem. Concr. Res., vol. 39, no. 9, pp. 787–797, Sep. 2009. [45] S. H. P. Cavalaro and a. Aguado, “Intrinsic scatter of FRC: an alternative philosophy to estimate characteristic values,” Mater. Struct., no. Cv, 2014. [46] Buratti, N., & Mazzotti, C. (2017). Creep Testing Methodologies and Results Interpretation. In Creep Behaviour in Cracked Sections of Fibre Reinforced Concrete (pp. 13-24). Springer, Dordrecht. [47] Gettu, R., Zerbino, R., & Jose, S. (2017). Factors Influencing Creep of Cracked Fibre Reinforced Concrete: What We Think We Know & What We Do Not Know. In Creep Behaviour in Cracked Sections of Fibre Reinforced Concrete (pp. 3-12). Springer, Dordrecht. [48] Pujadas, P., Blanco, A., Cavalaro, S. H., de la Fuente, A., & Aguado, A. (2017). Flexural Post-cracking Creep Behaviour of Macro-synthetic and Steel Fiber Reinforced Concrete. In Creep Behaviour in Cracked Sections of Fibre Reinforced Concrete (pp. 77-87). Springer, Dordrecht. Figure 1 - Diagram of the complete test procedure O w F 𝐹 𝑝 𝐹 𝑐 t O w t0 t t1 t 𝐹 𝐿 PHASE 1 PHASE 2 CREEP TEST RECOVERY Figure 2 - Pre-cracking of the beams in Phase 1 (a) and detail of the position of the LVDT at the lateral side of the beam (b) 𝒘𝒑 𝒇 CMOD LVDT 30mm 12mm 40mm 280mm 280mm a) b) Figure 3 - Side view of the frame for the creep test (a), creep frame before (b) and after (c) loading. fulcrum supports b) lever arm load cell steel bars c) a) Figure 10 - Evolution of ∆𝑤𝑐 𝑡 over time for specimens with 𝑤𝑝 𝑓 of 2.50 mm: PFRC (a and b) and SFRC c) and d) 0,0 1,0 2,0 3,0 4,0 5,0 6,0 7,0 8,0 025 50 75 100 125 150 ∆wct [mm] Time [days] S1/PF_2.50P8 S1/PF_2.50P9 0,0 0,5 1,0 1,5 2,0 2,5 3,0 3,5 4,0 010 20 30 40 50 60 70 80 90 100 110 ∆wc t [mm] Time [days] S2/PF_2.50P6 0,0 0,1 0,2 0,3 0,4 025 50 75 100 125 150 ∆wc t [mm] Time [days] S1/SF_2.50P6 0,0 0,1 0,2 010 20 30 40 50 60 70 80 90 100 110 ∆wc t [mm] Time [days] S2/SF_2.50P8 S2/SF_2.50P9 a) b) c) d) Figure 11 - Failure of S2/PF_2.50P6 affected by tertiary creep Figure 12 – Evolution of 𝜑(𝑡) for beams with PFRC (a and b) and SFRC (c and d) for 𝑤𝑝 𝑓 of 0.25 mm and 1.50 mm 0,0 1,0 2,0 3,0 4,0 5,0 6,0 025 50 75 100 125 150 Creep Coefficient 𝜑(𝑡) [-] Time [days] S1/PF_0.25P1 S1/PF_0.25P2 S1/PF_0.25P3 S1/PF_0.25P4 S1/PF_0.25P5 S1/PF_1.50P6 S1/PF_1.50P7 0,0 1,0 2,0 3,0 4,0 5,0 010 20 30 40 50 60 70 80 90 Creep Coefficient 𝜑(𝑡) [-] Time [days] S2/PF_0.25P1 S2/PF_0.25P2 S2/PF_0.25P3 S2/PF_0.25P4 S2/PF_1.50P5 0,0 0,2 0,4 0,6 0,8 1,0 1,2 010 20 30 40 50 60 70 80 90 Creep Coefficient 𝜑(𝑡) [-] Time [days] S1/SF_0.25P1 S1/SF_0.25P2 S1/SF_0.25P3 S1/SF_0.25P4 S1/SF_1.50P5 0,00 0,50 1,00 1,50 2,00 2,50 3,00 025 50 75 100 125 150 Creep Coefficient 𝜑(𝑡) [-] Time [days] S2/SF_0.25P1 S2/SF_0.25P2 S2/SF_0.25P3 S2/SF_0.25P4 S2/SF_0.25P5 S2/SF_0.25P6 S2/SF_1.50P7 a) b) d) c) Table 1. Composition of the FRC mixture (in kg/m3) Table 2 - Fiber characteristics provided by the manufacturers Table 3 - Characterization of the FRC at 28 days S1/PF S2/PF S1/SF S2/SF Average [MPa] CV % Average [MPa] CV % Average [MPa] CV % Average [MPa] CV % 𝐸𝑐𝑚 31150 1.69 - - 31597 1.08 30160 2.20 𝑓 𝑐𝑚 52.15 1.52 48.89 1.57 54.30 1.51 46.77 2.54 𝑓𝐿 4.61 2.19 4.22 2.66 3.73 8.57 3.76 7.96 𝑓𝑅,1 2.01 22.30 2.38 15.54 4.62 12.15 3.75 22.29 𝑓𝑅,2 2.25 28.53 2.93 20.89 5.09 13.77 4.24 17.91 𝑓𝑅,3 2.46 26.84 3.32 24.15 5.10 15.91 4.30 15.88 𝑓𝑅,4 2.48 23.47 3.49 27.40 4.87 14.08 4.17 15.68 Materials Characteristics PLASTIC FIBERS STEEL FIBERS S1/PF S2/PF S1/SF S2/SF Gravel (6/15 mm) Granite 520 520 520 520 Gravel (2,5/6 mm) Granite 400 400 400 400 Sand (0/3 mm) Granite 500 500 500 510 Cement CEM I 52,5 R 400 400 400 350 Filler Marble dust 260 260 260 300 Water - 170 178 168 178 Superplasticizer Adva® Flow 400 12 12 12 12 Fibers PF/SF 5 (PF) 5 (PF) 40 (SF) 40 (SF) Characteristic Unity PF SF Length (L) [mm] 48 50 Equivalent Diameter (d) [mm] - 0.62 Aspect ratio (L/d) [-] 44 83 Tensile strength (fy) [MPa] 550 1270 Modulus of elasticity (E) [GPa] 10 210 Number of fibers per kg [fibers] >35000 8100 Table 4. —Summary of loading conditions and pre-crack width SPECIMENS 𝒕 [days] 𝒘𝒑 𝒇 [mm] 𝑭𝒄 [kN] 𝛏 = 𝑭𝒄𝑭𝒑 ⁄ [%] S1 PF S1.PF_0.25P1 151 0.25 0.244 6.8 48.9 S1.PF_0.25P2 151 0.232 7.1 58.2 S1.PF_0.25P3 151 0.236 10.1 69.1 S1.PF 0.25P4 151 0.230 9.4 57.3 S1.PF_0.25P5 151 0.2516 9.8 60.5 S1.PF_1.50P6 151 1.50 1.507 9.1 50.0 S1.PF_1.50P7 151 1.507 6.5 50.4 S1.PF_2.50P8 151 2.50 2.536 9.5 54.0 S1.PF_2.50P9 151 2.532 8.8 48.6 SF S1.SF_0.25P1 151 0.25 0.336 14.5 53.9 S1.SF_0.25P2 151 0.332 14.6 61.6 S1.SF_0.25P3 151 0.363 14.7 69.8 S1.SF_1.50P4 151 1.50 1.578 16.3 52.9 S1.SF_2.50P5 151 2.50 2.746 16.2 49.5 S1.SF_2.50P6 151 2.825 16.2 47.5 S2 PF S2.PF_0.25P1 98 0.25 0.251 6.6 48.9 S2.PF _0.25P2 98 0.266 5.6 48.3 S2.PF_0.25P3 98 0.244 5.3 48.6 S2.PF_0.25P4 98 0.260 6.3 52.6 S2.PF_1.50P5 98 1.50 1.499 5.0 43.1 S2.PF_2.50P6 108 2.50 2.498 6.0 49.3 SF S2.SF_0.25P1 98 0.25 0.257 9.1 47.0 S2.SF_0.25P2 98 0.252 10.4 62.2 S2.SF_0.25P3 98 0.202 10.5 52.3 S2.SF_0.25P4 98 0.253 10.4 52.3 S2.SF_0.25P5 98 0.251 7.1 46.5 S2.SF_0.25P6 98 0.252 7.1 53.7 S2.SF_1.50P7 98 1.50 1.502 7.1 46.8 S2.SF_1.50P8 98 1.500 9.1 48.0 S2.SF_2.50P9 98 2.50 2.501 9.0 37.1