Full text
FURTHER INTO THE INFRARED WITH QUANTUM DOT PHOTODETECTORS Onur Özdemir ICFO – The Institute of Photonic Sciences Barcelona, 2021
Further Into the Infrared with Quantum Dot Photodetectors Onur Özdemir under the supervision of Prof. Gerasimos Konstantatos submitted this thesis in partial fulfillment of the requirements for the degree of Doctor of Philosophy in Photonics by the Universitat Politècnica de Catalunya Barcelona, 2021
Acknowledgements I am very grateful to have countless people that supported and guided me through this PhD experience. This has been more than a learning and research experience thanks to all of you. I am deeply thankful to my supervisor Gerasimos Konstantatos for making everything possible and giving me the opportunity to be a part of our amazing group. Thanks to his endless support and guidance, I always felt motivated and inspired to take on the challenges of the PhD and grew to become a confident researcher. My colleagues and friends in our constantly evolving FoN group deserve huge gratitude. Santanu and Nengjie were my first mentors, thank you for introducing me to this world. My FoN-QMantis-Qurv friends Shuchi and Yu, thanks to you for being there for me when I was regularly confused about anything related to chemistry. Francesco, Alberto, Sotirios and Laura thank you for the very scientific lunch discussions and occasional cheesecake from Badalona. A massive thanks to my friend and mentor Iñigo who taught me a lot in the lab and also how to be a good researcher, I am very fortunate to have someone like you. Huge thanks to my quantum queen Mariona, dai Shanti, always interesting Ignasi, brilliant Nima for being amazing. Thanks to Guy for being an awesome colleague, friend and a flatmate and helping me keep my sanity during lockdown! Thanks, Zafer for the long chats about anything and everything, Gaurav and Stephy for inspiring me on being motivated, Biswajit for his positivity and many thanks to Shanmukh, Avijit, Yongjie, Zhouran and Lucheng. I owe a huge thanks to all the ICFOnians and the people who make ICFO an enjoyable place. Thanks to Anne and all the HR for a warm welcome, all the NFL people including Luis, Javi and Johann that helped me a lot in the clean room, Vittoria for the help in the PPL, Carlos for making sure that ICFO keeps operational as well as electronic and mechanical workshops.
To all my friends that made Barcelona so much better, Alican, Inci, Gülçin, Kutlu, Ceren, Civan, Selda, thank you all. Thanks to my marvelous friends, Bahar and Zeynep for sharing the first years of Barcelona experience with me. And thanks to Derya for being the first person to proof-read my thesis and all the simit. For the amazing cover photo, I’d like to thank Артём. Most importantly, I want to thank my family. Their huge support made this possible. Thank you for always being there for me.
i Table of Contents TABLE OF CONTENTS I ABSTRACT III RESUMEN V LIST OF ACRONYMS VII 1 - INTRODUCTION 1 1.1 - Colloidal Quantum Dots 2 1.2 - Thesis Objectives and Outline 5 2 - PHOTODETECTOR BASICS 6 2.1 - Types of Photodetectors 6 2.1.1 - Thermal Detectors 6 2.1.2 - Photon Detectors 7 2.2 - Figures of Merit 8 2.3 - Noise Mechanisms in Photodetectors 10 2.4 - Background Limited Infrared Detection (BLIP) Limit 12 3 - HYBRID PHOTODETECTORS UTILIZING PBS QDS AND TMDCS 14 3.1 - Layered TMDCs 15 3.2 - TMDC – QD Hybrid Photodetectors 18 3.3 - Hybrid Photodetector Device Structure and Fabrication 18 3.4 - Electrical Characterization of Hybrid Photodetectors 22 3.5 - Optical Characterization of Hybrid Photodetectors 24 3.6 - Band Diagrams and Discussion 27 3.7 - Reference Devices 30 3.8 - Summary 34 4 - MOS2 – PBSE QD HYBRID PHOTODETECTORS FOR EXTENDED SWIR DETECTION 36 4.1 - PbSe Colloidal Quantum Dots 36 4.2 - PbSe-based Photodetector 38 4.3 - Hybrid Photodetectors with MoS2 and PbSe QDs 39 4.4 - Summary 44
ii 5 - ROBUST HIGH N-DOPING IN PBS QD FILMS AND PHOTODETECTORS UTILIZING INTRABAND TRANSITIONS 47 5.1 - Doping of Quantum Dots 47 5.2 - Highly n-doped PbS QD Films 49 5.3 - Optical Intraband Response of High-doped PbS QD Films 53 5.4 - Size-Dependent Intraband Transitions in Doped Films 55 5.5 - Occupation of the Conduction Level and Size-dependent Doping 58 5.6 - High n-doping at Low Temperatures and its Optical Characterization 61 5.7 - Low-temperature FET measurements of Doped Films 64 5.8 - Photodetectors Utilizing Intraband Transitions in High-doped PbS QDs 65 CONCLUSION 69 BIBLIOGRAPHY 72 LIST OF PUBLICATIONS 82
iii Abstract In the infrared, photodetectors are the key components in a wide-variety of applications such as thermal imaging, remote sensing, spectroscopy with newer technologies added to the list such as LiDAR and deep tissue imaging. As the demand for photodetectors increase with a shift towards longer wavelengths, we need high-performance, scalable and low-power consuming alternatives to current infrared photodetector technologies. Colloidal Quantum Dots (CQDs) are nanoscale-sized semiconductors with quantum-confined charges in all 3 dimensions. They can be synthesized in solution and can easily be deposited onto a desired substrate as a quantum dot (QD) film which allows easy integration with current silicon-based technologies. QDs are efficient light absorbers and their bandgap can accurately be tuned by controlling their size during synthesis. Lead chalcogenide QDs, such as PbS and PbSe, have tunable bandgaps covering the near-infrared (NIR) and short-wave infrared (SWIR) up to 3 µm, making them ideal sensitizers for photodetectors. In this thesis, we utilize PbS QDs with an excitonic bandgap around 1.8 µm in combination with 2-dimensional transition metal dichalcogenides (TMDCs) to form hybrid photodetectors operating in the infrared. With their layered structure similar to graphene and semiconducting character, TMDCs have outstanding electronic properties. Incorporating few-layers of TMDCs in our PbS QD detectors allows fast and efficient charge transfer from the QDs to the photodetector contacts through the TMDC layer, boosting detector responsivity. By combining PbS QDs with two types of TMDCs, WS2 and MoS2, we are able to reach detectivities exceeding 1012 Jones at room temperature with a response up to 2 µm. Probing further into the infrared, we extend the spectral response of our hybrid detectors up to 3 µm by utilizing narrower-bandgap PbSe QDs with MoS2 layers. After a careful analysis and using strategies such as oxide-isolation of metallic contacts, we reached detectivities of 7.7 x 1010 Jones at 2.5 µm at RT. With their
iv low-noise and high responsivities, our detectors improve the potential of hybrid detectors and demonstrate a performance comparable to commercial detectors without the need of external cooling, costly vapor deposition techniques or complex integration with silicon technology. Broadening the reach of PbS QDs even further, even beyond the limit of their bulk bandgap, up to 9 µm by using a novel doping method, we demonstrate the first PbS QD intraband photodetectors. Having developed this air-stable high n-doping method for PbS QDs, observation of intraband transitions taking place between the first two conduction levels becomes possible. These intraband transitions have lower energies compared to the bandgap, opening up another degree of freedom in tunable optical response of our QDs between 6-9 µm. We study how the doping works across a wide range of QD sizes and at different temperatures. Our photodetectors utilizing the intraband transitions in highly-doped PbS QD films have detectivities approaching 105 Jones. To sum up, we demonstrated lead chalcogenide QD based photodetectors with improved performance and spectral responses progressively shifting deeper into the infrared. Our TMDC-QD hybrid detectors reveal the potential of these systems as alternatives to commercial detectors. Whereas, surpassing the bandgap limit with high doped QDs and intraband transitions opens up new ways to realize optoelectronic devices further in the infrared.
v Resumen En el infrarrojo, los fotodetectores son los componentes clave en una amplia variedad de aplicaciones, como escaneo térmico, teledetección, espectroscopia, además de otras tecnologías más nuevas, como LiDaR o escaneo de tejidos profundos. A medida que aumenta la demanda de fotodetectores con aplicaciones hacia longitudes de onda más largas, necesitamos alternativas de alto rendimiento, escalables y de bajo consumo de energía a las tecnologías actuales de fotodetectores infrarrojos. Los puntos cuánticos coloidales (CQD) son semiconductores de tamaño nanométrico con portadores de carga confinados cuánticamente en las 3 dimensiones. Se sintetizan en solución y se pueden depositar fácilmente sobre cualquier sustrato en forma de película de puntos cuánticos (QD) que permite una fácil integración con las tecnologías actuales basadas en silicio. Los QDs son absorbentes de luz eficientes y sus bandas prohibidas se pueden ajustar controlando su tamaño durante la síntesis. Los QDs de calcogenuro de plomo, como PbS y PbSe, tienen bandas sintonizables que cubren el infrarrojo cercano (NIR) y el infrarrojo de onda corta (SWIR) hasta 3 µm, lo que los convierte en sensibilizadores ideales para fotodetectores. En esta tesis, utilizamos PbS QD con una banda prohibida excitónica de 1,8 µm en combinación con dicalcogenuros de metales de transición bidimensionales (TMDCs) para formar fotodetectores híbridos que operan en el infrarrojo. Con su estructura en capas similar al grafeno y su carácter semiconductor, los TMDC tienen propiedades electrónicas sobresalientes. La incorporación de unas pocas capas de TMDC en nuestros detectores de PbS QD permite una transferencia de carga rápida y eficiente desde los QDs a los contactos del fotodetector a través de la capa TMDC, lo que aumenta la capacidad de respuesta del detector. Al combinar PbS QD con dos tipos de TMDCs, WS2 y MoS2, podemos alcanzar detectividades superiores a 1012 Jones a temperatura ambiente con una respuesta de hasta 2 µm.
Chapter 1 - Introduction 4 modifying the surface chemistry of the QDs. There is a plethora of ligands14 to choose from depending on the application and that specific QD size and material. Careful selection of an appropriate ligand is therefore crucial to the performance of the final device and affects factors such as the doping, mobility, trap density and electron affinity.9 In the infrared, there are various choices of semiconductors that can be synthesized as CQDs. A summary of these materials and their wavelength span can be seen in Figure 1.2-a. Materials such as HgTe CQDs can span a wide range of wavelengths; however, Hg containing compounds can potentially lead to health and environmental concerns. Less toxic alternatives such as lead chalcogenides (such as PbS, PbSe, PbTe) are focus of active research. Safer materials such as Ag2Se CQDs15,16 are also considered as alternatives to Hg and Pb-based CQDs.17 Figure 1.2 – (a) Spectral sensitivity ranges for several CQDs in the SWIR-NIR region. Adapted from ref 18.(b) Normalized absorption for several different sized PbS CQDs. As the diameter of the CQDs increase from 1.8 nm to 6.4 nm, excitonic absorption peak redshifts, allowing tunable photoresponse. In this thesis, main focus will be on two lead chalcogenide CQDs: PbS and PbSe. These CQDs are synthesized using a Schlenk line by a hot-injection method where precursors are injected into organic solvents at elevated temperatures. Control of the CQD size and size distribution is achieved by factors such as injection temperature, type of precursors, stabilizing surfactants and reaction time. During the reaction stages of nucleation and growth are separated and individually controlled to obtain the desired optical properties. In the end, a CQD solution is obtained in an organic solvent with each CQD capped with long ligand chains for colloidal stability. Figure 1.1-b shows PbS CQDs with various diameters using the synthesis described above. 0.6 0.8 1 2 3 4 5 6 7 8 Wavelength ( m) Si Ge PbS PbSe PbTe InAs InSb Ag2Se HgTe ab 600 800 1000 1200 1400 1600 1800 Wavelength (nm) 0 0.5 1 1.5 2 Normalized Absorption (arb. u.) Increasing CQD diameter
5 1.2 - Thesis Objectives and Outline The main objective of the thesis is to develop and optimize photodetectors in the short-wave to mid-infrared range with high performance, low noise and low cost. We want these detectors to be easily integrated with the silicon-based technology and to be alternatives to the current commercial detectors without the need of costly and bulky external cooling systems. To reach these goals, we use lead chalcogenide CQDs in combination with TMDCs in the short-wave infrared range. For photoresponse in the mid-infrared, we utilize a novel doping technique on lead sulfide CQDs to allow low-energy transitions in the CQDs. This thesis is organized as follows: Chapter 2 provides the basics of photodetectors. Different types of photodetectors and their principles of operation are discussed. Fundamental limits on detector performance are laid out and noise in photodetectors are investigated. Figures of merit on assessing the performance of these detectors are introduced. Chapter 3 presents novel hybrid photodetectors with PbS QDs and two different types of TMDCs. An introduction on TMDCs and their properties are discussed. Following that, hybrid photodetectors utilizing MoS2 and WS2 combined with PbS QDs are introduced. Their characterization and performance assessment concludes the chapter. Chapter 4 advances the hybrid photodetectors further into the infrared. With PbSe QDs and an MoS2 layer below, we are able to obtain response up to 3 µm. The performance of the device is further improved by oxide-isolation of contacts, resulting in higher detectivity. Chapter 5 introduces a novel method to obtain high-doped PbS QD films and presents another degree of freedom in controlling the absorption of QDs. The method is analyzed in detail and studies on doping versus QD size and temperature are presented. Photodetectors using the highly-doped QD film is presented that operate in the MIR-LWIR.
6 2 - Photodetector Basics In almost every imaging system that we use today, we have photodetectors. As the interest shifts from visible wavelengths to infrared, we need new technologies to cover the IR. But before that, a deep understanding of photodetector operating principles is needed. This chapter will cover the basic types of photodetectors, how we assess their performance and their fundamental limits. 2.1 - Types of Photodetectors Depending on their operation principle, photodetectors are mainly divided into two categories: thermal detectors and photon detectors. When a photon hits the active material of the detector and it heats up the material therefore causing a change in conductivity, then it can be classified as a thermal detector. If that photon excites an electron and creates an electron-hole pair that can be collected by the terminals of the device and extracted as photocurrent, then the device can be classified as a photon detector. In this thesis, I will focus on photon detectors; however, a brief description of thermal detectors is provided for comparison purposes. 2.1.1 - Thermal Detectors There are various types of thermal photodetectors including bolometers, thermopiles and pyroelectric detectors. The active materials in these types of devices respond to a temperature change and different mechanisms are used to detect the temperature change as an electrical signal. In bolometers, the conductivity of the active materials changes due to heating of the material and this can be detected using a differential circuitry, such as a Wheatstone bridge. Thermopiles on the other hand, are thermocouples usually connected in series. They operate on the basis of differential temperature change converted into a voltage difference due to thermoelectric effect. And pyroelectric detectors output signal when they detect a change in temperature and widely used in sensors.
7 Thermoelectric photodetectors are generally slow when compared to photon detectors. Their response is usually in the millisecond range. They are usually much noisier than photon detectors, but they are cheaper to manufacture and they don’t usually require active cooling.4 Compared to photon detectors, they have a flatter spectral response. 2.1.2 - Photon Detectors These types of detectors operate on the principle of photon absorption creating mobile charge carriers. Generally, they can be divided into photoconductor and photovoltaic photodetectors. Photoconductors change their resistivity when light hits them. They are essentially radiation-sensitive resistors. If the energy of the incident photon is larger than the bandgap of the material, then the photon gets absorbed and an electron-hole pair is created. These carriers are then swept to the contacts by the applied bias voltage. Change in the current across terminals of the photodetector is then detected as signal. Photocurrent in a photoconductive detector can be expressed as: 𝐼!" =#𝑞𝜂𝐴Φ#𝐺 Equation 2.1 Where 𝑞 is the fundamental charge, 𝜂 is the external quantum efficiency, 𝐴 is the detector area, Φ# is photon flux density incident on the device and 𝐺 is photoelectric current gain. Suitable active material selection is important as photocurrent depends on 𝜂 , the external quantum efficiency. This value includes the effects such as surface reflection and scattering that internal quantum efficiency misses. Photovoltaic detectors have a built-in electric field that separates the photogenerated charges. This field may arise as a result of a p-n junction, heterojunction, Schottky barrier or a metal-insulator-semiconductor junction. As a result of a built-in electric field, in the depletion region charges are accelerated, thus making photovoltaic detectors faster. Photocurrent for a photovoltaic detector can be expressed with the same equation for photoconductors, except that the gain factor is taken as one (apart from avalanche photodetectors which can have gain factors larger than one).
Chapter 2 – Photodetector Basics 8 Figure 2.1- Comparison of photoconductive and photovoltaic mechanisms in photon detectors. (a) Schematic of a photoconductive detector with contacts (yellow) and the corresponding band diagram (b) that shows the photogenerated charges. EC and EV signify conduction and valence band energies in the semiconductor. (c) The schematic for a photovoltaic detector using a p-n junction as the active area and corresponding band diagram in (d). 2.2 - Figures of Merit Considering many different architectures and materials being used in photodetectors, we need generally accepted and quantitative measures to compare and assess their performance. These performance metrics are reported in many photodetectors and they are used in this thesis extensively. External Quantum Efficiency. The EQE, or 𝜂 , is the ratio of number of charge carriers collected by the detector to the number of photons incident on the active area. In contrast to internal quantum efficiency (IQE), which considers the number of absorbed photons by the active material, EQE takes into account all kind of external losses such as reflection and scattering, therefore EQE is always smaller than IQE. Ideally, it can take values between 0 and 1 unless there is an internal gain mechanism. Responsivity. The responsivity of a photodetector is the ratio of electrical output over incident light power on the detector. Electrical output can either be a change in electrical potential or current; therefore, responsivity has units of volts per watt V/W
9 or amperes per watt A/W. Current responsivity of a photon detector can be expressed as: 𝑅=#𝐼$%&!%& 𝑃'()'*+(& =#𝜆𝑞𝜂 ℎ𝑐#𝐺 # Equation 2.2 where 𝜆 is the wavelength, 𝑞 is the electron charge, 𝜂 is the EQE, # ℎ is the Planck’s constant, 𝑐 is the speed of light and 𝐺 is photoconductive gain that may be greater than 1 for some photoconductive photodetectors and is limited to 1 for photovoltaic ones. Noise Equivalent Power. The noise equivalent power (NEP) is the incident power on the detector generating a signal output equal to the noise output. Stated another way, the NEP is the signal level that produce a signal-to-noise ratio (SNR) of one.4 It can be thought as the minimum light power that the detector can respond to and distinguish from noise. In terms of current output response and responsivity, it can be expressed as: 𝑁𝐸𝑃=#𝐼( 𝑅 Equation 2.3 where 𝐼( is the noise current in Amperes. NEP has units of Watts. In some sources, NEP is normalized to the electrical bandwidth of the measuring equipment 19, as both noise power and NEP depend on measurement bandwidth and is indicated by 𝑖( . In that case bandwidth-normalized-NEP has units of W Hz1/2. Detectivity and Specific Detectivity. Detectivity (D) is simply defined as the inverse of NEP. However, this metric by itself does not include the effects of area or bandwidth. Therefore, specific detectivity or normalized detectivity denoted as 𝐷∗ is proposed by R. Clark Jones in 1953 to establish a common ground in comparing photodetectors with different areas, different bandwidths and noise properties.20 It is defined as: 𝐷∗=#√𝐴𝐵 𝑁𝐸𝑃=#𝑅√𝐴𝐵 𝐼( Equation 2.4 where 𝐴 is the device area and 𝐵 is the electrical bandwidth. 𝐷∗ has units of Jones and is mainly used in this work to compare and characterize photodetectors of
Chapter 2 – Photodetector Basics 10 varying architectures. In SI units, Jones is expressed as cm Hz1/2 W-1. If bandwidthnormalized-NEP ( 𝑖( ) is to be used in defining 𝐷∗ , then the equation becomes: 𝐷∗=#𝑅√𝐴 𝑖( Equation 2.5 Although specific detectivity ( 𝐷∗ ) is proposed as a comparison metric, it still does not include the measurement conditions of bias voltage, temperature or modulation frequency. These parameters should be specified when 𝐷∗ is being reported. Also, as the responsivity of a photodetector depends on the excitation wavelength, 𝐷∗ also depends on it, which needs to be reported as well. 2.3 - Noise Mechanisms in Photodetectors Thermal and photon detectors have different detection mechanisms and therefore different sources of noise. Thermal detectors are generally limited by temperature fluctuation noise arising from radiant power exchange with a radiating background. On the other hand, photon detectors are generally limited by generation– recombination noise arising from photon exchange with radiation background.21 For this thesis, I will focus on the noise mechanisms of photon detectors. In a photon detector, there are optical and electronic noise sources. Electronic noise is present in almost all electronic devices and is related to the movement of electrons in the detector circuit. Optical noise arises from the statistical nature of photons and their probabilistic interaction with the active material, exciting carriers in the detector. There are mainly four types of noise mechanisms in photoconductors: shot noise, 1/f noise, thermal noise and generation-recombination noise. Shot Noise. This type of noise arises due to the probabilistic nature of particles. Photon emission from a source does not happen at a constant stable rate, but it is a probabilistic process that is characterized by Poisson statistics and is especially pronounced when number of particles are low. The same type of noise applies to electrons that are passing through a potential barrier, like a p-n junction or a grain boundary. Each electron has an independent random possibility of passing through the junction at any given time, described by Poisson statistics. As a consequence, shot noise scales with the mean current that passes through the circuit. For electrons, it can be expressed as:
11 𝐼#"$& =#42𝑞𝐼-+.(𝐵 Equation 2.6 where 𝐼-+.( is the average current passing through the circuit and 𝐵 is the bandwidth of the measurement equipment. Shot noise is white; i.e., it is independent of frequency. Photonic shot-noise is prominent in ultraviolet or visible detectors, but it is shadowed by background radiation for detectors operating in infrared above about 1.5 µm wavelength at room temperature.22 Thermal Noise. Also called Johnson noise, this type of noise is associated with the random thermal motion of carriers in resistors and not with the fluctuating number of carriers. This type of noise is present in all electronic equipment even when there is no bias voltage applied. It can be expressed as: 𝐼&"+/-.0 =#26𝑘𝑇𝐵 𝑟 Equation 2.7 Where 𝑘 is Boltzmann’s constant, 𝑇 is the temperature in Kelvins and 𝑟 is the resistance of the device. This type of noise is ideally white. Generation-Recombination Noise. In photon detectors, when a finite bias is applied through the contacts, carrier density fluctuates due to random generation and recombination attributed to lattice vibrations. Because of that, at a given time it is unlikely that there will be exactly the same number of charge carriers in the free state at succeeding instances of time and that is observed as changes in conductivity and therefore changes in photocurrent in the device. Expressions for G- R noise change in low and high bias regimes and according to the doping level of the conductor. This type of noise is generally dominant in intermediate frequencies and is less pronounced in high frequencies.4 1/f Noise. Sometimes called flicker noise, this type of noise is dominant at lower frequencies. The origins of this noise are still not clear; however, it is observed consistently in many electronic systems. In general, 1/f noise appears to be associated with the presence of potential barriers at the contacts, interior, or surface of the semiconductor. Reduction of 1/f noise to an acceptable level is an art that depends greatly on the processes employed in preparing the contacts and surfaces.4 Power spectral density of this type of noise is observed in measurements as an inverse power law with respect to frequency:
Chapter 2 – Photodetector Basics 12 𝑃𝑆𝐷#∝#1 𝑓1 Equation 2.8 where k is a constant that depends on the device. 2.4 - Background Limited Infrared Detection (BLIP) Limit The performance of the detectors, especially in the mid and long-infrared, is limited due to background emitting at infrared wavelengths, due to finite temperature of the environment. Therefore, photodetectors operating at these wavelengths cannot distinguish between the background emission and the intended source. Even if the quantum efficiency is maximized and other sources of noise are minimized so that the system is not electronic-noise limited, background radiation puts a limit on the performance of infrared photodetectors. As the temperature of the environment changes, the bounds of the limit also change; in a cold environment background emission will be reduced so the detectors can have a higher limit. Background radiation can be modelled as a blackbody source at a certain temperature, emitting in all directions. Planck modelled this emission as: 𝑄(𝜆,𝑇2)=# 2𝜋𝑐 𝜆3#(𝑒") 415! 6−1) Equation 2.9 where #𝑄 is the blackbody photon emittance (in units of photons m-3 s-1) and expressed in terms of 𝑇2 as the background temperature in K, 𝑐 as the speed of light, ℎ as Planck’s constant and 𝑘 as Boltzmann’s constant.23 We can see how the value for 𝑄 changes with respect to temperature in Figure 2.2. Assuming that we have a photovoltaic detector operating in infrared so that the detector is photonnoise limited (not electronic-noise limited), we can express the BLIP limit on detectivity 𝐷∗ as: 𝐷2789(9;) ∗=# 𝜆4𝜂 ℎ𝑐42Φ2 Equation 2.10 where Φ2 is the total background photon flux density reaching the detector, obtained by integrating 𝑄 with respect to wavelength to account for all the different energy photons. For a photoconductive detector, this limit is lower as both generation and
13 recombination take place in the same spatial location; therefore, additional recombination noise. Photoconductive BLIP limit becomes: 𝐷2789(9=) ∗=# 𝜆4𝜂 2ℎ𝑐4Φ2 Equation 2.11 If we assume a perfect detector with 𝜂=1 with a field of view of 180o, the curves in Figure 2.2 are obtained. In the visible, BLIP limit may not be important; however, infrared photodetectors face a significant upper limit with room temperature BLIP limit of about 2x1010 Jones at 14 µm for photoconductors. Figure 2.2 – Blackbody photon emittance at different temperatures (left) and the resulting BLIP limits on detectivity (D*) of the photodetectors in the infrared. Photoconductive (PC) are expressed as solid lines and photovoltaic (PV) limits are expressed as dashed lines. Once the background-limited performance is reached, the only detector parameter that can influence a detector’s performance is the quantum efficiency, 𝜂 . For QD- based photodetectors there is another important parameter besides 𝜂 that effects the BLIP limit: size uniformity. An ensemble of QDs with little size distribution between individual QDs will have a higher optical absorption coefficient than an ensemble with a wider size distribution. And reduced optical absorption in QDs results in an increase in the normalized dark current and a reduction in detectivity.24 1 4 7 10 13 16 19 22 25 Wavelength (µm) 10 20 10 22 10 24 10 26 10 28 10 30 Blackbody Photon Emittance (photons m -3 s -1 ) 80 K 300 K 400 K 1 4 7 10 13 16 19 22 25 Wavelength (µm) 10 10 10 11 10 12 10 13 10 14 Detectivity (Jones) PC Limit at 80 K PC Limit at 300 K PC Limit at 400 K PV Limit at 80 K PV Limit at 300 K PV Limit at 400 K
Chapter 3 – Hybrid Photodetectors Utilizing PbS QDs and TMDCs 20 the Raman shifts correspond to a layer thickness of 4-5 layers.52 Belonging to the same family of TMDCs, WS2 has similar vibrational modes. For WS2 flakes, E12g peak starts at 352.1 cm-1 in monolayer WS2 and goes to 348.7 cm-1 in its bulk form and the A1G peak goes from 417.5 cm-1 to 419.1 cm-1. For the WS2 flakes that we observed, the vibrational Raman shifts correspond to a thickness of 3-4 layers (Figure 3.5-b).53 Figure 3.5 - Raman spectra for MoS2 (a) and WS2 (b) flakes after exfoliation measured with a 532 nm laser. Vibrational modes E12G and A1G are depicted in the figures next to their corresponding peaks. Next step in the device fabrication is the spincoating of appropriately sized PbS QDs on the TMDC FET devices. For that, CQDs are synthesized as follows and spincoated onto the device with a proper ligand exchange procedure. PbS CQDs of 1.8 µm exciton wavelength are synthesized following a previously reported multi-injection method.54 Briefly, 0.45 g lead oxide (PbO), 100 mL 1- octadecene (ODE) and 3.8 mL oleic acid were mixed and degassed overnight at 90ºC under vacuum. After the degassing, the solution was placed under Argon, the reaction temperature was set to 115ºC and a solution of 55 µL hexamethyldisilathiane ((TMS)2S) in 3 mL ODE was quickly injected. After 6 minutes, a second solution of 135 µL (TMS)2S in 12 mL ODE was dropwise injected with a rate of 0.75 mL/min. After this second injection, the heating was stopped, and the solution was let to cool down naturally to room temperature. CQDs were purified three times by precipitation with acetone and ethanol and redispersing in anhydrous toluene. Finally, the CQD concentration was adjusted to 30 mg/mL in toluene and the solution was bubbled with N2 for 30 minutes to avoid oxidation. 300 350 400 450 500 550 600 Raman Shift (cm-1) Intensity (arb. u.) 200 300 400 500 600 700 Raman Shift (cm-1) Intensity (arb. u.) abWS2 flake MoS2 flake E2g 1 peak E2g 1 peak A1g peak A1g peak Chapter 3. Properties and characterization of 2D TMDCs 3.3(a) presents the two phonon modes and their atomic displacements for two layers of MoS 2 .TheE 1 2G phonon corresponds to a strong in-plane vibrational mode with spectral appearance around 386 cm 1 for monoloayer MoS 2 .TheA 1G mode originates from an out-of-plane mode and peaks around 405 cm 1 . With increasing flake thickness, E 1 2G red shifts and A 1G blue shifts, and both slowly approach their bulk phonon modes for flake thicknesses of more than 5 layers [66]. Following a classical model for coupled harmonic oscillators, an increase (blue shift) in both peak frequencies would have been expected due stronger restoring forces by adjacent planes. However, theoretical DFT calculations have revealed that neighboring layers of MoS 2 enhance the dielectric screening of long-range coloumb interactions, resulting in a decrease in the E 1 2G frequency [67]. Although the reported peak positions vary and depend on factors like temperature and the substrate [68,69], the di↵erence between the peaks of the two modes is a precise diagnostic tool for determination of the number of layers as depicted in Figure 3.3(b). The frequency di↵erence has been correlated with AFM data to calibrate the Raman system on the used substrates. In agreement with literature, a striking di↵erence is noticed for the first 1-4 layers. This di↵erence decreases with increasing thickness, thus limiting its accuracy for thicker flakes. Figure 3.3: Few layer MoS2raman modes. (a) Schematic of the two characteristic and detectable raman modes, E 1 2G and A 1G , of few-layer MoS 2 . The atomic displacement is a↵ected by neighboring layers, leading to a thickness dependence of the raman spectrum. (b) Peak frequency and frequency di↵erence between the characteristic raman modes for 1 - 5 layers. Extracting the di↵erence is an accurate tool to estimate the number of layers for few-layer MoS2flakes. Apart from AFM and Raman, additional reliable methods like the measurement of photoluminescence spectra o↵er insight into the quality and number of layers of the 2D sample under investigation. The continuous change in the band structure 26 Chapter 3. Properties and characterization of 2D TMDCs 3.3(a) presents the two phonon modes and their atomic displacements for two layers of MoS 2 .TheE 1 2G phonon corresponds to a strong in-plane vibrational mode with spectral appearance around 386 cm 1 for monoloayer MoS 2 .TheA 1G mode originates from an out-of-plane mode and peaks around 405 cm 1 . With increasing flake thickness, E 1 2G red shifts and A 1G blue shifts, and both slowly approach their bulk phonon modes for flake thicknesses of more than 5 layers [66]. Following a classical model for coupled harmonic oscillators, an increase (blue shift) in both peak frequencies would have been expected due stronger restoring forces by adjacent planes. However, theoretical DFT calculations have revealed that neighboring layers of MoS 2 enhance the dielectric screening of long-range coloumb interactions, resulting in a decrease in the E 1 2G frequency [67]. Although the reported peak positions vary and depend on factors like temperature and the substrate [68,69], the di↵erence between the peaks of the two modes is a precise diagnostic tool for determination of the number of layers as depicted in Figure 3.3(b). The frequency di↵erence has been correlated with AFM data to calibrate the Raman system on the used substrates. In agreement with literature, a striking di↵erence is noticed for the first 1-4 layers. This di↵erence decreases with increasing thickness, thus limiting its accuracy for thicker flakes. Figure 3.3: Few layer MoS2raman modes. (a) Schematic of the two characteristic and detectable raman modes, E 1 2G and A 1G , of few-layer MoS 2 . The atomic displacement is a↵ected by neighboring layers, leading to a thickness dependence of the raman spectrum. (b) Peak frequency and frequency di↵erence between the characteristic raman modes for 1 - 5 layers. Extracting the di↵erence is an accurate tool to estimate the number of layers for few-layer MoS2flakes. Apart from AFM and Raman, additional reliable methods like the measurement of photoluminescence spectra o↵er insight into the quality and number of layers of the 2D sample under investigation. The continuous change in the band structure 26 Chapter 3. Properties and characterization of 2D TMDCs 3.3(a) presents the two phonon modes and their atomic displacements for two layers of MoS 2 .TheE 1 2G phonon corresponds to a strong in-plane vibrational mode with spectral appearance around 386 cm 1 for monoloayer MoS 2 .TheA 1G mode originates from an out-of-plane mode and peaks around 405 cm 1 . With increasing flake thickness, E 1 2G red shifts and A 1G blue shifts, and both slowly approach their bulk phonon modes for flake thicknesses of more than 5 layers [66]. Following a classical model for coupled harmonic oscillators, an increase (blue shift) in both peak frequencies would have been expected due stronger restoring forces by adjacent planes. However, theoretical DFT calculations have revealed that neighboring layers of MoS 2 enhance the dielectric screening of long-range coloumb interactions, resulting in a decrease in the E 1 2G frequency [67]. Although the reported peak positions vary and depend on factors like temperature and the substrate [68,69], the di↵erence between the peaks of the two modes is a precise diagnostic tool for determination of the number of layers as depicted in Figure 3.3(b). The frequency di↵erence has been correlated with AFM data to calibrate the Raman system on the used substrates. In agreement with literature, a striking di↵erence is noticed for the first 1-4 layers. This di↵erence decreases with increasing thickness, thus limiting its accuracy for thicker flakes. Figure 3.3: Few layer MoS2raman modes. (a) Schematic of the two characteristic and detectable raman modes, E 1 2G and A 1G , of few-layer MoS 2 . The atomic displacement is a↵ected by neighboring layers, leading to a thickness dependence of the raman spectrum. (b) Peak frequency and frequency di↵erence between the characteristic raman modes for 1 - 5 layers. Extracting the di↵erence is an accurate tool to estimate the number of layers for few-layer MoS2flakes. Apart from AFM and Raman, additional reliable methods like the measurement of photoluminescence spectra o↵er insight into the quality and number of layers of the 2D sample under investigation. The continuous change in the band structure 26 Chapter 3. Properties and characterization of 2D TMDCs 3.3(a) presents the two phonon modes and their atomic displacements for two layers of MoS 2 .TheE 1 2G phonon corresponds to a strong in-plane vibrational mode with spectral appearance around 386 cm 1 for monoloayer MoS 2 .TheA 1G mode originates from an out-of-plane mode and peaks around 405 cm 1 . With increasing flake thickness, E 1 2G red shifts and A 1G blue shifts, and both slowly approach their bulk phonon modes for flake thicknesses of more than 5 layers [66]. Following a classical model for coupled harmonic oscillators, an increase (blue shift) in both peak frequencies would have been expected due stronger restoring forces by adjacent planes. However, theoretical DFT calculations have revealed that neighboring layers of MoS 2 enhance the dielectric screening of long-range coloumb interactions, resulting in a decrease in the E 1 2G frequency [67]. Although the reported peak positions vary and depend on factors like temperature and the substrate [68,69], the di↵erence between the peaks of the two modes is a precise diagnostic tool for determination of the number of layers as depicted in Figure 3.3(b). The frequency di↵erence has been correlated with AFM data to calibrate the Raman system on the used substrates. In agreement with literature, a striking di↵erence is noticed for the first 1-4 layers. This di↵erence decreases with increasing thickness, thus limiting its accuracy for thicker flakes. Figure 3.3: Few layer MoS2raman modes. (a) Schematic of the two characteristic and detectable raman modes, E 1 2G and A 1G , of few-layer MoS 2 . The atomic displacement is a↵ected by neighboring layers, leading to a thickness dependence of the raman spectrum. (b) Peak frequency and frequency di↵erence between the characteristic raman modes for 1 - 5 layers. Extracting the di↵erence is an accurate tool to estimate the number of layers for few-layer MoS2flakes. Apart from AFM and Raman, additional reliable methods like the measurement of photoluminescence spectra o↵er insight into the quality and number of layers of the 2D sample under investigation. The continuous change in the band structure 26 Mo S W S
21 Transmission electron microscopy (TEM) images of the dots can be seen in Figure 3.6-a. Analysis of TEM images reveal an average diameter of the QDs is 8.03 ± 1.67 nm. The diameter and the excitonic absorption peak match closely with the model developed by Moreels et al.55 and also from previous experimental works in our group.56 After the synthesis of PbS CQDs, we measured their absorption spectra in toluene, using a Cary 5000 Spectrophotometer. Pure toluene is taken as a background (indicated with a black dashed line in Figure 3.6-b) and CQD solution is diluted in the same toluene for absorption measurements. The absorption curve can be seen in Figure 3.6-b and shows a clear exciton peak near 1.8 µm. Figure 3.6 – (a) TEM images of the CQDs used in this study. The scale bar on the bottom left indicates 20 nm. (b) Spectral absorption of the PbS CQDs in toluene after synthesis (blue curve). Absorption of toluene is indicated by a dotted black line. To form the hybrid device and coat the CQDs on TMDC transistors as a film, it is necessary to decrease the distance between QDs and to passivate their surfaces with a proper ligand exchange treatment. Previous research in our group on PbS solar cells suggest that a mixed ligand treatment of ZnI2 and MPA (zinc iodide and 3-mercaptopropionic acid) for large sized PbS QDs suppress trap state density, possess higher mobilities and result in a larger electron affinity when compared to 1,2-ethanedithiol (EDT) ligand treatment; which is a common ligand used with PbS QD films.57 Therefore, this mixed ligand treatment has been our choice for our devices. PbS QD films are deposited using a layer-by-layer spin-coating process under ambient conditions at 2500 rpm. ZnI2+MPA ligand solution is prepared in methanol (25x10-3 M ZnI2 with 0.01% MPA v/v). Dropping CQD solution (in toluene) following by ligand solution and methanol for washing the excess unbound ligands, layer-by-layer deposition is performed on the TMDC transistors. The process is repeated 4 times. Resulting thickness of the QD film is measured with a profilometer ab 800 1000 1200 1400 1600 1800 2000 2200 Wavelength (nm) Absorption (arb. u.) 20 nm 20 nm
Chapter 3 – Hybrid Photodetectors Utilizing PbS QDs and TMDCs 22 as 85 nm. Optical microscope images of the final devices can be seen in Figure 3.4- c,e. 3.4 - Electrical Characterization of Hybrid Photodetectors Figure 3.7 – IDS-VGS curves in dark for WS2 based device (a) and MoS2 based device (b) in different stages of fabrication in logarithmic scale. Arrows correspond to the direction of the gate voltage sweep. To characterize the electrical properties of hybrid detectors, we performed measurements in ambient conditions using an electromagnetically isolated probe station and a semiconductor analyzer (Agilent B1500A) with a 4-probe connection. Measurements of source-drain current (IDS) versus back-gate voltage (VGS – applied through the doped-Si underneath) are shown in Figure 3.7 with a bias voltage (VDS) of 1V applied between the source-drain contacts. In TMDC FETs, as the VGS is swept between -40V and 20V, we can see a clear off-state induced by the electric field through the TMDC by the gate electrode. In the off-state, the current passing through the transistor channel (IDS) is around 1-10pA as indicated by the dashed curve and is limited by the measuring equipment. After the QD layer is deposited on the TMDC transistors, off-state currents increase in both MoS2 and WS2 based devices. In MoS2 based devices, this can be linked to the presence of sulfur vacancies that create high density of localized states and an uncontrolled doping resulting in an increase of the off-state currents.58 A similar mechanism can also be present in WS2 based devices. Off-state dark currents in both WS2 and MoS2 based devices are in a similar range in the final devices, around 5-10nA. We can calculate the field-effect mobility, µ, of the charges by fitting the linear region of the IDS-VGS curves, under the short channel approximation as: (2)
23 𝜇=𝑑𝐼>? 𝑑𝑉@? #𝐿 𝑊𝐶$A𝑉>? Equation 3.1 where L and W are the length and width of the TMDC channel and Cox is the capacitance of the oxide layer. Cox is taken as 1.28x10-8 F cm-2 for a thickness of 285 nm of SiO2. The slopes of the IDS-VGS curves are calculated when the device is in the on (conducting, non-depleted) state. A significant hysteresis in the curves can be seen in all devices which can be linked to atmospheric adsorption and trapped charges; an issue being addressed by many groups.59,60 Due to hysteresis, forward and backward field-effect mobilities are different and are tabulated in Table 3.1. Forward curve is defined as starting with a negative VGS and increasing to positive voltages, while backward curve is the opposite. For the remainder of this chapter, we will only consider backward mobilities. Device Forward Mobility (cm2/Vs) Backward Mobility (cm2/Vs) MoS2 17.74 21.93 MoS2 + QDs 5.10 7.27 WS2 19.38 30.16 WS2 + QDs 6.19 12.42 Table 3.1 - Mobilities of the devices in various steps of fabrication. Forward and backward values are extracted from Figure 3.7 and calculated using Equation 3.1 Upon QD deposition, for WS2 based device, field-effect mobility decreased from 30.2 to 12.4 cm2/Vs; and for the MoS2 based device, it decreased from 21.9 to 7.3 cm2/Vs. In both devices hysteresis in the transfer curves decreased significantly after the QD layer is deposited. This can be attributed to a decreased interaction of the TMDC layers with atmospheric adsorbates. In TMDC based photodetectors due to high on/off ratios that these materials inherently possess, noise levels are low; resulting in high specific detectivities (D*). Therefore, a careful analysis of this low noise in the off-state is necessary. For our devices, we measured the noise power spectral density (PSD) by two different methods. Firstly, by analyzing the Fourier transform (FFT) of the IDS and secondly, by measuring the noise at different frequencies with a lock-in amplifier under the same biasing conditions. For the first method, noise spectra are obtained as FFT of dark current traces spaced 4 ms apart. The second method uses a lock-in based setup: Zurich Instruments MFLI with a 2-channel low noise power source Keysight B2962A.
Chapter 3 – Hybrid Photodetectors Utilizing PbS QDs and TMDCs 24 Figure 3.8 - Noise characteristics of hybrid devices in dark conditions. Measurements obtained by taking the FFT of the dark current traces (scattered dots) and by the lock-in (hollow dots and lines) match closely. Shot noise limits are indicated by horizontal lines for WS2 (green) and MoS2 (blue) based devices. 1/f behavior (flicker noise) is indicated by dotted red lines as a guide to the eye. Noise PSDs for both devices are shown in Figure 3.8 and they are similar in terms of magnitude and shape. Both FFT and lock-in methods give similar results. In low frequency range, up to approximately 5 Hz, the devices exhibit 1/f behavior (flicker noise, calculated to be 1/f1.7), indicated by dotted red lines. 3.5 - Optical Characterization of Hybrid Photodetectors Figure 3.9 - Responsivity versus incident light power on the photodetector active area, measured by using a 1310 nm laser. We first started optical characterization of our devices by measuring the responsivity of our photodetectors under infrared illumination. These measurements are performed in the same probe station as the electrical characterizations using a fiber-
25 coupled 1310 nm laser with adjustable power. VGS is swept to obtain maximum responsivity. In order to measure the laser power density incident on our devices, we used a Ge detector in combination with a 25 µm diameter circular aperture right before the detector. Figure 3.9 shows the responsivity of our devices with respect to increasing laser power. We observe a decrease in responsivity as the incident light power increases. As shown by Kufer et al.48 TMDC-QD hybrid photodetectors become less responsive in high illumination conditions, due to direct charge transfer from QDs. Photogenerated carriers in the QDs induce a reverse electric field, effectively lowering the built-in field.61 Charge carrier recombination is therefore accelerated at the interface with the resulting drop in responsivity. At an incident laser wavelength of 1310 nm, WS2 and MoS2 based devices have a maximum responsivity of 510 A/W and 103 A/W respectively. Similar to graphene–PbS QD hybrid photodetectors27, our hybrid photodetectors benefit from an internal gain mechanism, boosting responsivity. This photoconductive gain originates from photogenerated electrons in the QD layer being transferred to the high-mobility TMDC layer and circulating in the detector circuitry multiple times while holes are trapped inside the QDs. This yields to an internal gain, which is determined by the ratio: 𝐺=𝜏0'B+&'-+ 𝜏&/.(#'& # Equation 3.2 where tlifetime is the electron-hole recombination lifetime and ttransit is the carrier transit time through the contacts. tlifetime values can be extracted from time response of the detectors (Figure 3.10) and ttransit can be calculated as: 𝜏&/.(#'& =𝐿C 𝜇𝑉>?# Equation 3.3 where L is the length of the device (5 µm in our devices). We calculated the gain for WS2 based device as approximately 107 and for the MoS2 based device it is about 8.7x105.
Chapter 3 – Hybrid Photodetectors Utilizing PbS QDs and TMDCs 26 Figure 3.10 – Photoresponse decay times of the photodetectors, and time constants extracted from the decay curves. Photoresponse speed is another critical figure for many photodetector applications. We measured the response speed of our detectors using a 1310 nm laser. As the laser is turned off, exponential decay of the photocurrent can be seen in Figure 3.10 with different time constants. MoS2 based devices operate faster than WS2 based ones with a time constant of about 0.032 s to 0.2 s. These values are in range of previously reported hybrid devices and a detailed analysis will be provided in the following section. The final step is to characterize the spectral responsivity of our devices across the SWIR-NIR region. We performed these spectral responsivity measurements using a fiber coupled supercontinuum laser (SuperKExtreme EXW-4, NKT Photonics) in the same probe-station setup under same biasing conditions. During these measurements, we have adjusted the power of the laser such that the incident light power on the device for that wavelength is kept constant in order to rule out any effects from the power-dependent responsivity that these devices exhibit.
27 Figure 3.11 – Spectral responsivity (y-axis on the left) and detectivity (D*) (y-axis on the right) for the two types of hybrid devices in the 800 – 2400 nm range. Figure 3.11 shows the responsivity of our devices in the 0.8 – 2.4 µm range, with a clear excitonic peak at around 1.8 µm in both devices. At this wavelength, responsivity reaches 1442 A/W and 202 A/W for WS2 and MoS2 based devices respectively. The detectivity, D*, is then calculated by using Equation 2.5. Our WS2 and MoS2 devices exhibit detectivities of 1.0x1012 and 2.8x1011 Jones, respectively, at room temperature with their photoresponse reaching up to 2.1 µm. Previously reported PbS-based hybrid photodetectors, while having high detectivities (7x1013 Jones), have only achieved photoresponse up to 1.5 µm.46 The only other hybrid devices to achieve responsivity up to 2.1 µm were based on HgTe, with detectivities in the same order as our WS2 based devices.50 3.6 - Band Diagrams and Discussion Constructing band diagrams are essential in properly analyzing our photodetectors and to better understand their operating mechanism. In this work we have used exfoliated TMDC layers and therefore the sizes of our flakes have an area in order of 30-100 µm2. With these small sizes, traditional techniques such as ultraviolet photoelectron spectroscopy (UPS) measurements are not possible. In addition to that, in hybrid devices PbS QD layer thickness exceeds the penetration depth of UPS, preventing a detailed analysis of the interface between TMDC-QDs. Our analysis of the band diagrams are based on reported values for TMDCs, UPS values of the PbS QD film by itself and observations on our measurements in Figure 3.7. (1)
Chapter 3 – Hybrid Photodetectors Utilizing PbS QDs and TMDCs 28 Figure 3.12 - Band Alignments of the materials used in our devices for (a) WS2 based and (b) MoS2 based devices. CB and VB indicate conduction and valence bands respectively. Ef indicates the Fermi level denoted by dashed lines. The shaded gray areas in (a) indicates the uncertainty of the exact position of the band edges for WS2. (c, d) Band diagrams including band bending for our hybrid devices, following the discussion in this chapter. We have used UPS values from the literature while determining the bandgap and electron affinity energies. Reports of experimental UPS measurements of exfoliated TMDC flakes show that valence band of WS2 and MoS2 lies below 5.99 and 5.49 eV from the vacuum level respectively.62 Some other UPS measurements performed on chemically grown WS2 denote the valence band edge around 5.65 eV below the vacuum level.63 For this reason, in Figure 3.13-a, we included and uncertainty in the valence and conduction band edges for WS2, as the exact position is still not settled yet. For the bandgaps of few-layers of TMDCs, we have used the experimental values from other groups; for MoS2 and WS2 they are approximately 1.39 eV 64 and 1.42 eV 65 respectively. As for the PbS QDs, we have used -5.0 eV for the valence band maximum (VBM), as obtained from previous UPS measurements from our group for QDs similar to the ones employed here.56 The conduction band maximum (CBM) has been obtained by adding the measured optical bandgap to the VBM.
29 Figure 3.13 - IDS-VGS curves of the hybrid photodetectors in linear scale for (a) WS2 and (b) MoS2 based devices. In both cases, curves shift to the right after QD deposition, which is indicated by an arrow. Observations on IDS-VGS curves give clues about the band alignment in the TMDCQD heterojunction. In Figure 3.13 the curves that are previously presented in logarithmic scale in Figure 3.7 are plotted in linear scale and magnified to better observe the threshold voltages. Threshold voltage is the VGS above which the transistor starts conducting and goes into the on-state. In both cases, before QD deposition, we can see that the threshold voltages lie in the lower voltages whereas after QD deposition, threshold voltages shift to higher voltages. This indicates that the hybrid transistor system is less n-doped than the bare TMDC transistor system, which suggest electron transfer from the TMDC to the QDs upon junction of the two materials. Therefore, the Fermi level (Ef) of the QDs must be below the Fermi levels of TMDCs before they are combined. The shift in the threshold voltages is larger in the case of MoS2 as compared to WS2. This suggests there is a larger difference in Fermi levels between MoS2 layers and QD layers than in WS2. We know that: (i) the Fermi level of the QDs must be lower than that of the TMDCs, (ii) the Fermi level of MoS2 is higher than that of WSs; and (iii) both WS2 and MoS2 are n-type and highly conductive, therefore, for each of them, we assume that the Fermi level should not be more than 3 or 4 times kT below the CBM. In addition, we have calculated the Fermi level of our PbS CQD film to be approximately 0.085 eV below the CBM, as explained below. In order to accurately pin the Fermi level of the PbS QD film, we have fabricated transistors without an underlying TMDC layer. These results can be found in the following section 3.2.5. For our discussion, we borrow some results from the IDS-VGS of these devices that utilize the same PbS QDs. With these curves, we have been able to obtain the electron population, n, in our PbS CQD film, following the method
36 4 - MoS2 – PbSe QD Hybrid Photodetectors for Extended SWIR Detection In the previous chapter, we have explored hybrid photodetectors with MoS2 and WS2 and PbS QDs. In this chapter, we extend our understanding of hybrid photodetectors and utilize it for another kind of QD sensitizer, lead selenide. This lead chalcogenide is similar to PbS; however, with slight differences that allows us to probe further into the infrared. We were able to extend the bandwidth of our hybrid photodetectors up to almost 3 µm at room temperature. 4.1 - PbSe Colloidal Quantum Dots PbSe in its bulk form is a narrow bandgap semiconductor with a bandgap of 0.278 eV (4.46 µm) at room temperature which is smaller than of bulk PbS (0.42 eV).2 It has an exciton Bohr radius of 46 nm which is larger than PbS Bohr radius of 20 nm.68 These properties alone make PbSe a great candidate for infrared optoelectronics once it is made into QDs. PbSe QDs are first reported as early as 1997 in a phosphate glass host.69 Then, liquid-phase syntheses are developed which led to better control over QD size and size.70 In this study, we use a synthesis developed by Yu et al. with modifications to increase yield and get a narrow size distribution.71 We have obtained PbSe CQDs with an excitonic peak at 2.5 µm using a similar Schlenk line procedure as PbS with hot injection method. 2 mmol PbO, 15 mmol oleic acid, and 10 mL 1-octadecene were mixed in a three-neck flask and heated at 100°C under vacuum for 1 hour to form lead oleate, stirring at 650 rpm. Then, the solution was placed under Argon, the temperature was raised to 180°C and a solution of TOP-Se was quickly injected (2 mmol Se, 200 µL DPP and 1 mL TOP). After 3 minutes of reaction under these conditions, a second solution of trioctylphosphine-Se (2 mmol Se in 2 mL trioctylphosphine) was injected dropwise.
37 Immediately after this second injection, the reaction was quenched with a water bath. Once at room temperature, CQDs were separated by centrifugation and redispersed in anhydrous toluene. The addition of 10 µL butylamine was necessary to redisperse the precipitate. Subsequently, the product was washed for three times with a mixture of acetone/ethanol and finally redispersed in anhydrous toluene, adjusting the concentration to 30 mg/ml. The final solution was bubbled with nitrogen to avoid the oxidation of the material. Figure 4.1 – PbSe CQDs in tetrachloroethylene solution after synthesis. (a-b) TEM images of the QDs with two different magnifications. Scale bars are identified on the lower left corner. (c) Absorption spectra of the QDs in solution with a prominent excitonic peak around 2.5 µm indicated with a solid line. Absorption of the solvent tetrachloroethylene is indicated with a dotted line. (d) Size distribution of the QDs obtained from the TEM images with an average diameter of 8.6 ± 0.57 nm. Figure 4.1 summarizes the PbSe CQDs after synthesis. High resolution TEM images show non-agglomerated QDs with a uniform distribution. The crystalline structure of the individual QDs can be seen in the images. The absorbance spectra in Figure 4.1-c shows an excitonic peak around 2.5 µm (0.5 eV) with another high-energy peak around 1.8 µm (0.69 eV). The CQDs are capped with oleic acid and is in a solution of tetrachloroethylene to get rid of any parasitic absorption from the solvent. A histogram of size distribution of the QDs are extracted from the TEM images. The CQDs have an average diameter of 8.6 ± 0.57 nm and compared to the Bohr radius a b 50 nm 5 nm 7.5 8 8.5 9 9.5 10 QD Diameter (nm) 0 5 10 15 20 25 30 Count c d 1500 1750 2000 2250 2500 2750 3000 Wavelength (nm) Absorption (arb. u.)
Chapter 4 – MoS2 – PbSe QD Hybrid Photodetectors for Extended SWIR Detection 38 for PbSe of 46 nm, we can say that our CQDs are in the quantum confinement regime. 4.2 - PbSe-based Photodetector After obtaining the PbSe QDs, we have utilized them in a simple photodetector architecture as a starting point without any TMDC layer. A schematic of the device can be seen in Figure 4.2-a. Figure 4.2 – (a) Schematic of the photodetector with only PbSe QDs. (b) IDS - VGS curve of the detector in dark. The arrows show the direction of VGS sweep. 1V of VDS is applied between the contacts. We have used a back-gated architecture using doped-Si and SiO2 (285 nm). We patterned source and drain electrodes using photolithography and Ti/Au (3/50 nm) deposition. The distance between the contacts is 5 µm. We then spincoated several layers of PbSe QDs onto the substrate. To replace the oleic acid ligands on the surface of the PbSe CQs and get a close-packed, high-mobility film we used 1,2- ethanedithiol (EDT) during spincoating. This layer-by-layer process is repeated 2 times to obtain a final PbSe QD film thickness of around 50 nm. Electrical and optical characterization of the device was performed in an electromagnetically isolated probe station at room temperature with 4-probe connections to a semiconductor analyzer. In Figure 4.2-b, IDS-VGS curve is depicted with 1V of bias between source and drain contacts. We can see that the QD film is highly conductive and the electric field is not able to induce a remarkable modulation in IDS. The film demonstrates a p-type character with a field-effect hole mobility of 0.96 cm2V-1s-1 calculated using Equation 3.1. VGS Si SiO2 PbSe QD film VDS IR radiation -40 -20 0 20 40 VGS (V) 1.782 1.784 1.786 1.788 IDS (A) 10-3 VDS = 1V ab
39 Figure 4.3. (a) Responsivity of the photodetector to a 1310 nm laser with respect to incident light power. Grey line is a guide to the eye. (b) Noise current spectral density of our device in dark between 1-100 Hz. Grey line is a guide to the eye and shows the 1/f component of noise. (c) Spectral responsivity between 1250-3000 nm. The peak arising from the excitonic peak of PbSe around 2.5 µm can be seen clearly. Figure 4.3-a shows the responsivity of our photodetector as the incident light power increases with a maximum of 0.08 A/W at low light power. The measurement is performed with a power-adjustable 1310 nm laser incident on the active area of the detector. It shows a logarithmic decrease as the sensitizing traps in QDs are saturated.48 Spectral response of the detector is measured by a monochromator based setup and the responsivity between 1250 – 3000 nm is plotted in Figure 4.3- c. A peak around 2.5 µm is visible that corresponds to the excitonic peak of the QDs that corresponds to a responsivity of 0.055 A/W. Noise current spectral density (in) is measured in dark with a lock-in based setup using the same biasing conditions as the responsivity measurements. Typical 1/f component of noise can be seen in Figure 4.3-b. Detectivity (D*) can then be calculated using Equation 2.5. At 2.55 µm, our PbSe-only photodetector has a detectivity of 1.96 x 106 Jones at room temperature. 4.3 - Hybrid Photodetectors with MoS2 and PbSe QDs Two issues limit the performance of the PbSe-only photodetector: high dark current and low mobility of the PbSe film. In this section, we will address both issues and improve upon the performance of the detector. Firstly, we can utilize a TMDC layer underneath the QDs to take advantage of the high mobility of TMDCs and by forming a heterojunction to take advantage of the inherent gain mechanism that arises from this hybrid photodetector, as demonstrated and discussed extensively in the previous chapter. For that we utilized few-layers of MoS2 between the contacts underneath the PbSe QD layer. We chose MoS2 in this case over WS2 due to its closer conduction band alignment with PbSe QDs. The fabrication process is similar to the one described in the previous chapter; 100101102 Frequency (Hz) 10-11 10-10 Noise Current Density (A Hz-1/2 ) 4 6 8 10 Incident Light Power (W) 10-8 0.04 0.05 0.06 0.07 0.08 0.09 0.1 Responsivity (A/W) 1500 2000 2500 3000 Wavelength (nm) 0 0.05 0.1 0.15 Responsivity (A/W) VGS = 0V VDS = 1V = 1310 nm VGS = 0V VDS = 1V VGS = 0V VDS = 1V abc
Chapter 4 – MoS2 – PbSe QD Hybrid Photodetectors for Extended SWIR Detection 40 we exfoliated MoS2 layers from a bulk MoS2 on top of the Si/SiO2 substate and identified the flakes under a microscope followed by the lithography of source-drain contacts on both sides of the flake. We preserved the same architecture i.e., the same dimensions for the contacts and active area. We then spincoated PbSe QDs of about the same thickness as before (2 cycles of layer-by-layer spincoating, resulting in a thickness if around 50 nm) using the EDT ligand exchange. Figure 4.4 – (a) Schematic of the hybrid MoS2-PbSe photodetector. (b) IDS-VGS curves of the hybrid detector before (black curve, left y-axis) and after (orange curve, right y-axis) PbSe QD film deposition. Arrows indicate the direction of the VGS sweep with VDS = 1V. (c) Schematic of the hybrid detector with Al2O3 isolated source-drain contacts. (d) IDS-VGS curve of the contactisolated device before (black curve, left y-axis) and after (blue curve, right y-axis) PbSe QD film deposition. (e) Responsivity vs. light power for the hybrid (orange) and contact-isolated hybrid (blue) detectors to a laser of 1310 nm. (f) Noise current spectral density of both devices with lines as a guide to eye. Stars indicate the maximum detectivity (D*) for both devices at the a b VGS doped-Si SiO2 Au MoS2 Al2O3PbSe QDs IR light VGS doped-Si SiO2 Au MoS2 PbSe QDs IR light e c d f
41 exciton wavelength at RT with their corresponding y-axis on the right. Reprinted with permission from 72. Copyright 2021 American Chemical Society. A schematic of the MoS2-PbSe QD hybrid device can be seen along with the IDSVGS curves of that device at various stages of fabrication can be seen in Figure 4.4- a and b. A rectifying behavior arising from the MoS2 can be seen clearly. After PbSe QD deposition the rectification is preserved with off-state currents around 320 nA (at VDS = 1V), which is where the device will be operated to take advantage of the reduced dark current. The field effect electron mobility in the hybrid device is 16.5 cm2V-1s-1. As we have seen in the previous section with PbSe-only photodetector, we have a QD film that is very conductive. As we apply a bias voltage between source and drain contact, we expect a current passing through the MoS2 layer (which can be turned off with backgating) However, as the QD film itself is conductive, under the same bias, a significant amount of current passes through the QD film, that cannot be influenced by backgating. Therefore, in the hybrid device we observe a relatively high dark current which masks the photocurrent and reduces responsivity. To overcome this problem, we decided to isolate the source-drain electrodes by depositing an oxide barrier on them such that the electrodes are only in contact with the MoS2 layer below. This will ensure that dark current contribution from the QD film reduces and photogenerated carriers can still be transferred from the QDs to the MoS2 layer and then to the contacts. Figure 4.5- A summary of the fabrication of contact-isolated hybrid photodetector. Reprinted with permission from 72. Copyright 2021 American Chemical Society A quick summary of the fabrication process for the contact-isolated hybrid device can be seen in Figure 4.5. We chose Al2O3 as the oxide as it can be deposited uniformly onto the whole sample at low temperatures and good coverage. As usual, doped-Si SiO2 few-layer MoS2flakes doped-Si SiO2 Gold contacts doped-Si SiO2 doped-Si SiO2 Al2O3 deposition doped-Si SiO2 doped-Si SiO2 PbSe QDs Photoresist Lift-off a b c de f
Chapter 4 – MoS2 – PbSe QD Hybrid Photodetectors for Extended SWIR Detection 42 MoS2 flakes are transferred onto a Si/SiO2 substrate and regions of few-layer MoS2 are identified. Ti/Au contacts are patterned in each side of the flake to create an MoS2 transistor. Then, after another photolithography step, MoS2 flake is protected with photoresist. 5 nm of Al2O3 is deposited onto the whole sample using ALD at 80°C. Photoresist is then removed in hot acetone to reveal the MoS2. PbSe QDs are spincoated twice to reach a thickness of 50 nm. Source-drain contacts are then contacted for characterization by bigger pads far away from the active region where the same photoresist protection is performed (not shown in the schematic). A schematic of the contact-isolated device and the corresponding IDS-VGS curve can be seen in Figure 4.4-c and d. We can see that in the final device, off-state currents are down to 10 nA as a result of the oxide isolation process. We can still see the rectification behavior arising from MoS2 layer. The field effect electron mobility of the final device is calculated as 6.37 cm2V-1s-1. Figure 4.6 – (a) A schematic of the band alignment between few layers of MoS2 and PbSe QDs treated with EDT. (b) Band bending and charge transfer under illumination in the hybrid detector. In both hybrid devices, as we deposit PbSe QDs on top of MoS2 layer, we create a heterojunction with a built-in electric field. In order to better understand the dynamics of this junction, we performed UPS measurements for the PbSe QD film treated with EDT used on our devices. Valence band edge of the QDs lie at 4.54 eV below vacuum level with Fermi level 0.23 eV above it. Based on the optical absorption measurements of the QDs, bandgap is deduced to be 0.52 eV, which puts the conduction band at 4.02 eV below vacuum level. For MoS2, we utilized the values for few-layers from literature.64 The resulting band alignment in the heterojunction is sketched in Figure 4.6-a. Following a similar discussion as in the previous chapter, if we observe the IDS-VGS curves, we can see that the threshold voltage shifted towards higher voltages after -4.0 -4.5 -5.0 -5.5 Au MoS2 PbSe QDs CB VB Ef Energy (eV) MoS2 PbSe QDs CB VB Ef Energy (eV) a b - + - - - ++
43 QD deposition. Just as in the WS2-PbS detector in the previous chapter, this suggests electron transfer from the TMDC to the PbSe layer, resulting in band bending depicted in Figure 4.6-b. Under IR illumination, electron-hole pairs are generated in the PbSe QDs. Holes are trapped in the QDs while electrons move towards MoS2 and then to the contacts. This leads to the gain mechanism that we are familiar with from the previous chapter and boosts the responsivity as electrons move several times in the circuitry while holes are trapped until they recombine. Figure 4.4-e shows the responsivity of both the hybrid devices with respect to changing light intensity. Under 1310 nm laser light the hybrid device reaches responsivities around 23.5 A/W. For the isolated-contact hybrid device this value goes up to 192 A/W. At high light powers, the responsivity decreases in both cases as a result of the reverse electric field induced by high number of photogenerated carriers near the heterojunction.61 For the contact-isolated device this effect is more prominent as more photogenerated charges pass through the junction rather than reaching the contacts directly skipping MoS2. This results in an enhanced reverse electric field and manifests itself as a slightly steeper decrease with respect to increasing light power in the measurement. Noise current spectral densities (in) of both hybrid devices are measured and plotted in Figure 4.4-f. The 1/f behavior can be seen in both measurements with very similar dependence on frequency. Contact-isolated device has lower noise in across the frequencies measured. High responsivity and low noise in the contact-isolated device translates into higher detectivity. The detectivity of the hybrid device is 1.0 x 1010 Jones whereas the contact-isolated hybrid device has a detectivity of 7.7 x 1010 Jones at RT. Figure 4.7 – Spectral responsivity of the contact-isolated hybrid device between 1250-3000 nm with a peak around 2.5 µm, corresponding to the excitonic absorption of PbSe QDs. Detectivity (D*) corresponding the same measurement is plotted on the right axis. (b) Response speed of the same device to a laser of 1310 nm. Time constant is about 0.04 s as the laser illumination is switched off. Reprinted with permission from 72. Copyright 2021 American Chemical Society a b
Chapter 4 – MoS2 – PbSe QD Hybrid Photodetectors for Extended SWIR Detection 44 We measured the responsivity of the contact-isolated device up to 3 µm using the monochromator-based setup as before. Figure 4.7-a shows the resulting curve with the prominent excitonic peak around 2.5 µm originating from the PbSe QD layer. At 2.55 µm, responsivity reaches 137.6 A/W with a detectivity of 7.7 x 1010 Jones. Response speed of the contact-isolated device is also characterized by the 1310 nm laser and the semiconductor analyzer under the same biasing conditions and plotted in Figure 4.7-b. As the laser is turned off, photocurrent decreases exponentially with a time constant of 0.04 s. Photoconductive gain can then be calculated using Equations 3.2 and 3.3 where ttransit is calculated to be 3.9x10-8 s and gain is in the order of 106. 4.4 - Summary As in the previous chapter, to test the reproducibility of our devices, we fabricated and characterized several devices to see and the performance range of our hybrid photodetectors. These results are summarized below, in Table 4.1. Table 4.1 - A summary of the performance metrics of fabricated hybrid photodetectors. Device Max. Responsivity (A/W) Detectivity (Jones) MoS2 – PbSe Hybrid 1 41.9 1.0 x 1010 2 35.3 6.97 x 109 3 13.4 5.17 x 109 4 25.4 1.0 x 109 average 29.0 7.71 x 109 MoS2 – PbSe Hybrid with Al 2O3 isolation 1 137.6 7.7 x 1010 2 51.4 8.1 x 109 3 50.9 4.4 x 109 average 80.0 3.0 x 1010 The devices presented are fabricated on separate substrates following the same fabrication steps. On average, we can see that Al2O3 contact isolation helps increase the responsivity. The detectivities are in the range of 109-1010 Jones for the hybrid device without contact isolation and exceeds 1010 Jones after isolation. In this chapter, we demonstrated photodetectors based on PbSe QDs having an excitonic peak around 2.5 µm. We improved the performance of the photodetectors with a MoS2 layer to take advantage of the high mobility of such TMDCs and internal
45 electric field that drives the photogenerated charges towards MoS2. We isolated the source-drain contacts on both sides with Al2O3 to reduce the dark current from the conductive PbSe QD layer. In the end, we obtained a hybrid photodetector operating up to 3 µm with a detectivity of 7.7 x 1010 Jones at 2.55 µm at room temperature – highest reported to date for QD detectors in these wavelengths. These devices have the potential to be used in low-cost, high-performance applications without cooling and can be an alternative to current technologies. To place our hybrid devices in perspective, we summarized previously reported similar hybrid detectors operating at similar wavelength ranges in Table 4.2. Table 4.2 - Previously reported hybrid devices in the infrared consisting of TMDCs and QDs and some of their performance metrics. Active Material Spectral Coverage (nm) Responsivity (A/W) Detectivity (Jones) Response Time (s) Reference MoS2/PbS QD 400-1500 6 x 105 5 x 1011 0.3-0.4 48 MoS2/HgTe QD Vis-2200 ~103 ~1012 4 x 10-3 50 WS2/PbS QD 400-1500 14 3.9 x 108 2 x 10-4 49 WSe2/PbS QD 400-1400 2 x 105 7 x 1013 7 x 10-3 46 Bi2O2Se/PbSe QD Vis-2100 103 Not reported 4 x 10-3 73 MoS2/PbS QD 800-2100 202 2.8 x 1011 0.03 This work, Chapter 3 WS2/PbS QD 800-2100 1442 1.02 x 1012 0.2 This work, Chapter 3 MoS2/PbSe QD 1200-3000 41.9 1.0 x 1010 0.04 This work, Chapter 4 MoS2/PbSe QD (with Al2O3) 1200-3000 137.6 7.7 x 1010 0.04 This work, Chapter 4
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 52 Figure 5.3 – Transmission spectra of a PbS QD film treated with iodine before (red – undoped) and after (black – doped) alumina deposition. Both the bleach in the exciton signal and appearance of the intraband signal can be seen. Spectra are offset vertically for clarity. A notable property of high doping in PbS QDs is that both iodine and alumina are needed. Reports on similar lead chalcogenide QD films treated with sulfides93 and thiols94 that are infilled with low temperature alumina using ALD do not show intraband absorption or intraband bleaching. A combination of both iodine treatment and alumina is therefore essential. Strong n-doping with iodine and alumina is observed for similar systems by different groups as well. Abelson and coworkers observed doping and studied the effect of alumina on the QD film. Their X-ray diffraction and synchrotron grazing-incidence small-angle X-ray scattering (GISAXS) data shows that ALD infilling leaves the QD size, unit cell and spatial order of the QDs unchanged.95 They conclude that alumina does not affect the crystal structure but only passivates water and oxygen inside the film and prevents further oxidation. In our films we have confirmed that alumina does not stay on top of the QD film but it also infills the film by X-Ray Photoelectron Spectroscopy (XPS) measurements. Films are fabricated with a 3 nm alumina coverage in ALD. Prior to the measurement, the films are etched approximately 20-40 nm inside the XPS chamber and then the analysis is performed. 2p peak originating from aluminum is observed at that thickness, confirming the penetration of alumina inside the film.90
53 Figure 5.4 – Transmission spectra of the PbS QD film before and after doping. Series of measurements up to 67 days confirm long term stability of our doping in ambient. Stability of the doping play an important role to utilize these films in optoelectronic devices. We have tested the excitonic transmission of our samples up to 67 days. The samples are stored in ambient with constant exposure to light. In Figure 5.4, these measurements are plotted, conforming stability of at least 2 months in ambient. 5.3 - Optical Intraband Response of High-doped PbS QD Films While characterizing intraband transitions in various PbS films, we used Fourier transform infrared spectroscopy (FTIR) with a MIR source and a liquid nitrogen cooled MCT detector. We started with spincoating the PbS QDs with an EMII ligand exchange onto a double-side polished undoped silicon (10-20 Wcm) substrate of about 300 µm thickness. Unlike more common doped silicon wafers, undoped silicon is transparent between 0.1-0.75 eV range. We make sure that the films are thick enough to obtain a high signal to noise ratio. In our case, 5 repetitions of layer-by- layer deposition resulting in a 100 nm thick film is enough to achieve this. As there can be slight differences in thickness between samples due to the spincoating process, we measure the thickness of each PbS film with profilometer after fabrication. 11 S6: Stability test of the doped PbS CQD film Figure S6 : Series of absorption sepctra of doped PbS CQD film for a period of 67 days (solid lines). The sample was kept in ambient conditions with continuous exposure of ambient light. The respective undoped films is plotted for comparison (dash line). S7: X-ray Photoelectron Spectroscopy (XPS) in PbS QD solids We studied, with quantitative XPS analysis, the Pb/S ratio between the ad-hoc oleic capped PbS QD and the iodine treated PbS QDs in order to probe experimentally the substitution of I- in the (100) surface of the QDs. For that purpose, we used a series of PbS QD with different sizes. The small CQDs with band-edge absorption at 800nm do not have exposed sulfur rich surfaces, while starting with QDs absorbing at 1300 nm the (100) surface appears and the (100) surface increases in larger dots. Below we show the quantitative XPS fitting for both I- doped and oleic acid (OA) capped PbS QDs. The table summarizes the Pb/S in different QD sizes showing that in dots without the (100) surface the Pb/S ratio remains constant before and after the ligand exchange while the Pb/S is increased after the Iodide substitution in larger CQDs.
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 54 Figure 5.5 - Calculating the absorption in the heavily doped PbS QD films. (a) A schematic of the film, spincoated on top of an undoped silicon substrate. Incident light from the FTIR is taken as 1 and reflections and transmissions are subtracted from that to obtain the absorption in the film. (b) Example absorption spectra obtained by the measurements and calculated absorptions (c-d) Upper panel: Examples of calculated absorption spectra for different sized dots near the intraband (c) and interband (d) transition energies. Lower panel: Second derivative of the spectra above to accurately identify the peak position. Red lines indicate the gaussian fits to the data. We are able to obtain both transmission and reflection data in our FTIR system using a microscope setup. The setup is first calibrated with bare undoped-Si near energies where the absorption of the undoped-Si is negligible to make sure that transmission and reflection adds up to 100%. This may not always be the case for thin films, as the light reaches to the sample with high divergence and scattered light may affect the result 10-20%. When we are certain that the system is calibrated with only the light that reaches the sample with angles close to 90° to the film surface, we start the measurements for thin films. In Figure 5.5, a summary of the measurement method can be seen. We obtain the absorption in the film by: 𝐴B'0-I=1−𝑇-+.# −#𝑅-+.# −#𝐴#%J# Equation 5.1 undoped Si PbS QD film incident beam (1) transmitted beam (Tmeas) reflected beam (Rmeas) S-3 Figure S3. Example of the absorption measurement of a thin PbS layer in a sample as the one sketched in Figure S2. The absorption of the whole sample is obtained as: ܣ௦ ൌ ͳ െ ܶ௦ െ ܴ௦. The absorption of the PbS layer is obtained as: ܣ ൌ ܣ௦ െ ܣ௦௨௦. Figure S4. Typical absorption spectrum of the Si substrate used in this study. ab absorbed beam in the substrate (Asubs) absorbed beam in the film (Afilm) 7 Figure S3. FTIR transmission measurement of a 20-nm Al2O3 layer deposited by ALD on a lightO\GRSHGRKPāFPVLOLFRQVXEVWUDWH7KH$O2O3 transmission spectrum is obtained using a pristine silicon substrate as background sample. Al2O3 exhibits light absorption in the PUDQJH Figure S4. Examples of Gaussian fittings (red, dashed lines) used for obtaining the energies of the intraband (a), and first and second exciton transitions (b) in PbS CQD films. Dashed lines indicate the central energy of the Gaussian line shape. Insets indicate the electronic transition associated to each fitted peak. cd
55 where Tmeas is the measured transmission spectra for the substrate+film assembly, Rmeas is the measured reflection from the whole structure and Asubs is the absorption in the bare undoped-Si substrate that is measured prior to the measurement. In order to identify the peak location of the intraband and interband transitions for accurate analysis, we take the second derivative of the absorption curves in the film and fit gaussians to accurately pinpoint the energy, a method previously demonstrated by Cademartiri and coworkers.96 We repeat the process in the near infrared to fit the excitonic absorption peak for each film before and after alumina coating. Therefore, the bleach in the excitonic peak and its redshift can be identified for further analysis. To compare and quantify the strength of carrier transitions in our film, we also calculate the absorption coefficient, a. For the simple case of a thin slab of homogeneous material, a can be calculated by taking into consideration the multiple internal reflections that occur at the front and back air/sample interfaces, which increase the effective optical path.97 When the thin-film is deposited on a substrate, reflections taking place at every interface (refractive-index change), as well as absorption in the substrate, must be taken into account. For this case, a can also be analytically calculated assuming at≪1 98 where t is the thickness of the thin film. However, in all cases the refractive index of the sample or, alternatively, the fraction of reflected light in a single air/sample interface must be known. Because of the wavelength range in our study (5−9 μm), it was not possible for us to measure either of these values. Hence, we have calculated a using the model: 𝐴'(& =1−#𝑒Da& Equation 5.2 where Aint = Afilm/(1 − Rmeas). Aint represents the intrinsic absorption of the film irrespective of the external medium taking into account only the light that enters the film. Switching from the total absorption (Afilm) to the absorption coefficient (a) allows us to compare different samples with slightly different thicknesses, as we measure the exact thickness of the films with profilometry for each sample. 5.4 - Size-Dependent Intraband Transitions in Doped Films After obtaining high doping in PbS QDs, the next step is to study how the doping changes with respect to different sizes of QDs having different excitonic peaks. Figure 5.6-a summarizes the excitonic (interband) absorbance of different PbS QDs right after their synthesis. The QDs are freshly synthesized and capped with oleic acid and dispersed in toluene. We determine the diameter of the QDs by locating the peak energy in their absorbance spectra and using the experimentally fitted sizing curve proposed by Moreels and coworkers:
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 56 𝐸+A)'&$( =0.41+# 1 0.0252𝑑C+0.283𝑑 Equation 5.3 where Eexciton is the exciton energy and d is the dot diameter.55 Our dots have diameters in the range of 5.2 to 9 nm. Figure 5.6 – Intraband study of various sizes of doped PbS QD films. (a) Normalized excitonic absorption spectra of the QDs used in the study in toluene solution before film formation. QDs have diameter in the range of 5.2 – 9.0 nm. (b) Energies for the 1Sh -> 1Pe labeled as E2 and the excitonic 1Sh -> 1Se transition labeled as E1. Inset depicts a schematic of these transitions. Data points are the peak positions in absorption spectra as discussed in the text and lines are fits. (c) Normalized absorption (Afilm) for the intraband transitions at RT. As the dot size decreases, intraband absorption peak redshifts. (d) Energy of the intraband transition versus dot diameter. Markers indicate the peak of the gaussian fits to the data in (c) with an error bar of about 3meV. Red solid line is a fit to the markers. Black dashed line corresponds to the fit of E2 – E1 presented in (b). We then formed doped films on undoped-Si substrates and measured the absorption (Afilm) of the films as described previously. Figure 5.6-b shows the result of the fits to the absorption spectra for the 1Sh -> 1Se (E1) and 1Sh -> 1Pe (E2). We observed that after forming the film, the excitonic peak (E1) is redshifted as expected due to decreased distance between QDs leading to a slight loss of quantum confinement. We fitted these energies with: conventionally exploited interband transitions and can even be smaller than the band gap of the bulk counterpart, thus allowing exploitation of part of the electromagnetic spectrum forbidden for a given bulk SC material. To give an example of its potential, fine-tuning of and access to intraband transitions in CQDs could lead to photodetectors and light sources in the MWIR and LWIR 11 made of relatively high bandgap, cheap, and nontoxic materials, replacing the current technology based on epitaxially grown HgCdTe, InGaAs and GaInSb. 12 Consequently, work in this field is becoming more and more intense, and steady-state probing of intraband transitions has already been achieved in several materials. 13 However, until recently only mercury chalcogenide CQDs have exhibited stable high doping that allowed fabrication of intraband photodetectors. 11,14,15 Recently, robust heavy doping has been demonstrated in PbS CQD films, 16 enabling intraband absorption and photodetection in the MWIR and LWIR, 17 at energies smaller than the PbS bulk band gap. At this point, studies of the basic properties of intraband transitions in CQDs are needed to guide the development of intrabandbased devices and applications. In this work, we investigate the size and temperature dependence of intraband transitions in the CB of PbS CQDs. We report the intraband absorption coefficient of PbS QD films and discuss the size dependence of the oscillator strength of the first intraband transition in PbS QDs. RESULTS AND DISCUSSION PbS CQDs and Doped Films Used for the Study. Figure 1 shows absorbance spectra of the PbS CQDs used in this study, which evidence good control on the QD size (diameter) in the 5−9 nm range and low size dispersion. QD size has been obtained using the empirical model for oleic-acid capped QDs reported in ref 6after fitting the exciton energy in the absorbance spectra. After synthesis, we fabricated doped films following the method reported in ref 16. The films are spin-coated layer-by- layer on silicon substrates, exchanging the original oleic acid ligand with iodine. We use semi-insulating (lightly doped) silicon substrates throughout the whole study because the different measurements performed require transparency in the 1−12 μm range. After formation, the film is infiltrated and capped with alumina by atomic layer deposition, a method that has been proven to provide n-doping in PbSe 18 and ZnO 19,20 QDs. The resulting PbS CQD films are heavily n-doped (∼ 1019 cm−3) 16 and, consequently, exhibit steady-state intraband absorption in the CB. 17 Figure 2b shows the first two interband excitons in the doped films as a function of the dot diameter, d, obtained via analysis of the absorption spectra, as shown in Figure 2a. Note that for some samples, E2could not be accurately fitted, hence the reduced number of data points for E2in Figure 2b. We found that the first exciton is red-shifted in the doped films as compared to the as-synthesized solutions (Supporting Figure S1). We used this exciton-shift fingerprint as well as the doping level of the samples (discussed later and shown in Figure 4d) to discard oxidation of the dots before or during film formation, thus guaranteeing proper sample quality for further quantitative studies. We found that the samples that showed signs of oxidation (slight blue-shift of the first exciton) also exhibited lower doping levels. We have fitted the first exciton, E1(1Sh−1Se), and the second exciton, E2(1Sh−1Pe), with eqs 1and 2: =+ +Edd (eV) 0.41 1.50 4.2 12(1) with a fit correlation coefficient, R2> 0.99. =+ +Edd (eV) 0.41 3.09 1.4 22 (2) with R2> 0.99. The constant term 0.41 eV is the bulk band gap of PbS, Eg, at room temperature (RT). The size-dependent 1/d2 represents the confinement energy characteristic of particles Figure 1. Absorbance spectra, normalized to the maximum of the exciton peaks, of oleic-acid capped PbS CQDs dispersed in toluene. The QD diameter of the different solutions ranges between 5.2 and 9.0 nm. Figure 2. Interband absorption in heavily n-doped PbS CQD films. (a) Second-derivative analysis of the absorption spectrum. Vertical lines indicate the first three excitons. (b) Energy of the first two excitons, corresponding to lines 1 and 2 in (a) as a function of d. The lines are fits, as described in the main text. The inset illustrates the transitions of the first (red arrow) and second (blue arrows) excitons. Resulting from the n-doped character of the QDs, the measured E2originates exclusively from 1Sh−1Pe transitions and not from 1Ph−1Setransitions. ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7162 conventionally exploited interband transitions and can even be smaller than the band gap of the bulk counterpart, thus allowing exploitation of part of the electromagnetic spectrum forbidden for a given bulk SC material. To give an example of its potential, fine-tuning of and access to intraband transitions in CQDs could lead to photodetectors and light sources in the MWIR and LWIR 11 made of relatively high bandgap, cheap, and nontoxic materials, replacing the current technology based on epitaxially grown HgCdTe, InGaAs and GaInSb. 12 Consequently, work in this field is becoming more and more intense, and steady-state probing of intraband transitions has already been achieved in several materials. 13 However, until recently only mercury chalcogenide CQDs have exhibited stable high doping that allowed fabrication of intraband photodetectors. 11,14,15 Recently, robust heavy doping has been demonstrated in PbS CQD films, 16 enabling intraband absorption and photodetection in the MWIR and LWIR, 17 at energies smaller than the PbS bulk band gap. At this point, studies of the basic properties of intraband transitions in CQDs are needed to guide the development of intrabandbased devices and applications. In this work, we investigate the size and temperature dependence of intraband transitions in the CB of PbS CQDs. We report the intraband absorption coefficient of PbS QD films and discuss the size dependence of the oscillator strength of the first intraband transition in PbS QDs. RESULTS AND DISCUSSION PbS CQDs and Doped Films Used for the Study. Figure 1 shows absorbance spectra of the PbS CQDs used in this study, which evidence good control on the QD size (diameter) in the 5−9 nm range and low size dispersion. QD size has been obtained using the empirical model for oleic-acid capped QDs reported in ref 6after fitting the exciton energy in the absorbance spectra. After synthesis, we fabricated doped films following the method reported in ref 16. The films are spin-coated layer-by- layer on silicon substrates, exchanging the original oleic acid ligand with iodine. We use semi-insulating (lightly doped) silicon substrates throughout the whole study because the different measurements performed require transparency in the 1−12 μm range. After formation, the film is infiltrated and capped with alumina by atomic layer deposition, a method that has been proven to provide n-doping in PbSe 18 and ZnO 19,20 QDs. The resulting PbS CQD films are heavily n-doped (∼ 1019 cm−3) 16 and, consequently, exhibit steady-state intraband absorption in the CB. 17 Figure 2b shows the first two interband excitons in the doped films as a function of the dot diameter, d, obtained via analysis of the absorption spectra, as shown in Figure 2a. Note that for some samples, E2could not be accurately fitted, hence the reduced number of data points for E2in Figure 2b. We found that the first exciton is red-shifted in the doped films as compared to the as-synthesized solutions (Supporting Figure S1). We used this exciton-shift fingerprint as well as the doping level of the samples (discussed later and shown in Figure 4d) to discard oxidation of the dots before or during film formation, thus guaranteeing proper sample quality for further quantitative studies. We found that the samples that showed signs of oxidation (slight blue-shift of the first exciton) also exhibited lower doping levels. We have fitted the first exciton, E1(1Sh−1Se), and the second exciton, E2(1Sh−1Pe), with eqs 1and 2: =+ +Edd (eV) 0.41 1.50 4.2 12(1) with a fit correlation coefficient, R2> 0.99. =+ +Edd (eV) 0.41 3.09 1.4 22 (2) with R2> 0.99. The constant term 0.41 eV is the bulk band gap of PbS, Eg, at room temperature (RT). The size-dependent 1/d2 represents the confinement energy characteristic of particles Figure 1. Absorbance spectra, normalized to the maximum of the exciton peaks, of oleic-acid capped PbS CQDs dispersed in toluene. The QD diameter of the different solutions ranges between 5.2 and 9.0 nm. Figure 2. Interband absorption in heavily n-doped PbS CQD films. (a) Second-derivative analysis of the absorption spectrum. Vertical lines indicate the first three excitons. (b) Energy of the first two excitons, corresponding to lines 1 and 2 in (a) as a function of d. The lines are fits, as described in the main text. The inset illustrates the transitions of the first (red arrow) and second (blue arrows) excitons. Resulting from the n-doped character of the QDs, the measured E2originates exclusively from 1Sh−1Pe transitions and not from 1Ph−1Setransitions. ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7162 a b in a well under the effective mass approximation. The 1/dterm is an empirical observation required to fitE1and E2, as it was the case in previous studies, 6,21 indicating that corrections to this approximation are needed. In both transitions, the 1/d term is dominant over the quantum confinement one, as it is the case in as-synthesized PbS CQDs. 6 In fact, for E2, data can be fitted without the 1/d2term, in the 5 nm < d< 8 nm range, with R2> 0.99. However, the fact that the 1/d2term of E2is almost negligible in this size range is not particular of doped dots. Cademartiri et al. 21 showed that the second exciton in undoped PbS CQDs dispersed in solution deviates from the expected behavior for d> 5 nm, which caused E2to not be fitted to an equation of the form of eq 1 in the 4−7 nm size range. Therefore, although we expect eq 1 to be valid for d<5 nm, 6,21 we do not expect the same for eq 2. There is not a clear explanation for the peculiar size dependence of E2. Although it was a cause of controversy in the past, there is now a consensus that it corresponds to the 1Sh−1Peand 1Ph−1Setransitions. 22,23 These two have very similar energies due to the almost identical electron and hole effective masses in PbS, 24 as indicated in the inset of Figure 2b. Both transitions should be forbidden by symmetry. However, it has been shown that parity selection rules are relaxed in PbS QDs, allowing optical absorption features that do not conserve parity. 22 It has been discussed that breaking of the inversion symmetry of the wave function is needed to fully explain the optical absorption spectra of PbS QDs. 23 Ref 21 shows yet another higher-energy transition (seventh exciton) that exhibits a size dependence behavior similar to E2, with a sudden change in trend for d> 5 nm, and discusses the possibility that this transition originates from a separate corner of the Brillouin zone. Here, we propose another explanation for the sudden change in the size dependence of E2. It has been reported that the morphology of PbS QDs changes with size, evolving from an octahedral shape, for d< 3 nm, to a cuboctahedral shape, for d> 4 nm. 25 Small QDs have Pb-rich (111) facets, whereas in larger dots, S-rich (100) facets emerge. We argue that the change in morphology in large dots, having exposed sulfur atoms, may contribute to the formation of new states that modify the energy of the second (and possibly the seventh) interband transition. Size Dependence of the Intraband Transition. We have measured the absorption spectra of the intraband transitions in our films, Afilm, by means of transmission and reflection measurements via Fourier transform infrared spectroscopy. Our samples consist of a thin film (∼100 nm) of PbS QDs on top of a substrate (∼300 μm) of semi-insulating silicon, as sketched in Supporting Figure S2.Afilm is defined as =−−− A RTA1 film meas meas subs (3) where Rmeas and Tmeas are the measured transmission and reflection, and Asubs is the absorption of the substrate, which was previously characterized through reflection and transmission measurements (see Supporting Figure S3). Figure 3a shows that the intraband transition shifts to higher energies as the dot size decreases, owing to increased quantum confinement. Sharp features at around 0.14 and 0.15 eV arise from the differences (such as the amount of SiO2) in the reference silicon substrate and the substrate of each sample (see Supporting Figure S4). Below 0.13 eV, alumina contributes to absorption (Supporting Figure S5). The size dependence of the intraband energy, EIB, at RT is plotted in Figure 3b. We have fitted the results with eq 4: =−Edd (eV) 1.57 2.5 IB 2(4) with R2= 0.97. The negative value of the 1/d2term is expected, since we expect EIB to be equal to E2−E1(see eqs 1 and 2). For comparison, we have plotted E2−E1in Figure 3b. These results support the fact that, for all studied samples, the absorption peaks analyzed correspond to intraband transitions. As it was the case for E1and E2, the 1/dterm represents the dominant contribution to the size dependence of EIB. This will be useful later on for the analysis of the temperature dependence of EIB.As discussed previously, eq 2 is not valid for d< 5 nm, therefore, eq 4 should not be valid either. We do not know whether eq 2 and, hence, eq 4 still hold for d> 8.5 Figure 3. (a) Intraband absorption spectra of QDs of different sizes normalized to the peak maxima. (b) Energy of the intraband transition, at RT, as a function of the dot diameter. Data are obtained as the central energies of Gaussian fits of absorption spectra such as those presented in (a). The error bars are estimates of the uncertainty in the fits (±3 meV). The red solid line corresponds to eq 4. The black dashed line represents the energy difference between the second and first excitons. (c) Second confinement energy (E2−Eg) divided by the first confinement energy (E1−Eg) as a function of the first confinement energy. E2 (1Sh−1Pe) is obtained in two ways: directly from absorption spectra at RT (◇) and as EIB (1Se−1Pe)+E1(1Sh−1Se) at RT (●) and 98 K (☆). ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7163 in a well under the effective mass approximation. The 1/dterm is an empirical observation required to fitE1and E2, as it was the case in previous studies, 6,21 indicating that corrections to this approximation are needed. In both transitions, the 1/d term is dominant over the quantum confinement one, as it is the case in as-synthesized PbS CQDs. 6 In fact, for E2, data can be fitted without the 1/d2term, in the 5 nm < d< 8 nm range, with R2> 0.99. However, the fact that the 1/d2term of E2is almost negligible in this size range is not particular of doped dots. Cademartiri et al. 21 showed that the second exciton in undoped PbS CQDs dispersed in solution deviates from the expected behavior for d> 5 nm, which caused E2to not be fitted to an equation of the form of eq 1 in the 4−7 nm size range. Therefore, although we expect eq 1 to be valid for d<5 nm, 6,21 we do not expect the same for eq 2. There is not a clear explanation for the peculiar size dependence of E2. Although it was a cause of controversy in the past, there is now a consensus that it corresponds to the 1Sh−1Peand 1Ph−1Setransitions. 22,23 These two have very similar energies due to the almost identical electron and hole effective masses in PbS, 24 as indicated in the inset of Figure 2b. Both transitions should be forbidden by symmetry. However, it has been shown that parity selection rules are relaxed in PbS QDs, allowing optical absorption features that do not conserve parity. 22 It has been discussed that breaking of the inversion symmetry of the wave function is needed to fully explain the optical absorption spectra of PbS QDs. 23 Ref 21 shows yet another higher-energy transition (seventh exciton) that exhibits a size dependence behavior similar to E2, with a sudden change in trend for d> 5 nm, and discusses the possibility that this transition originates from a separate corner of the Brillouin zone. Here, we propose another explanation for the sudden change in the size dependence of E2. It has been reported that the morphology of PbS QDs changes with size, evolving from an octahedral shape, for d< 3 nm, to a cuboctahedral shape, for d> 4 nm. 25 Small QDs have Pb-rich (111) facets, whereas in larger dots, S-rich (100) facets emerge. We argue that the change in morphology in large dots, having exposed sulfur atoms, may contribute to the formation of new states that modify the energy of the second (and possibly the seventh) interband transition. Size Dependence of the Intraband Transition. We have measured the absorption spectra of the intraband transitions in our films, Afilm, by means of transmission and reflection measurements via Fourier transform infrared spectroscopy. Our samples consist of a thin film (∼100 nm) of PbS QDs on top of a substrate (∼300 μm) of semi-insulating silicon, as sketched in Supporting Figure S2.Afilm is defined as =−−− A RTA1 film meas meas subs (3) where Rmeas and Tmeas are the measured transmission and reflection, and Asubs is the absorption of the substrate, which was previously characterized through reflection and transmission measurements (see Supporting Figure S3). Figure 3a shows that the intraband transition shifts to higher energies as the dot size decreases, owing to increased quantum confinement. Sharp features at around 0.14 and 0.15 eV arise from the differences (such as the amount of SiO2) in the reference silicon substrate and the substrate of each sample (see Supporting Figure S4). Below 0.13 eV, alumina contributes to absorption (Supporting Figure S5). The size dependence of the intraband energy, EIB, at RT is plotted in Figure 3b. We have fitted the results with eq 4: =−Edd (eV) 1.57 2.5 IB 2(4) with R2= 0.97. The negative value of the 1/d2term is expected, since we expect EIB to be equal to E2−E1(see eqs 1 and 2). For comparison, we have plotted E2−E1in Figure 3b. These results support the fact that, for all studied samples, the absorption peaks analyzed correspond to intraband transitions. As it was the case for E1and E2, the 1/dterm represents the dominant contribution to the size dependence of EIB. This will be useful later on for the analysis of the temperature dependence of EIB.As discussed previously, eq 2 is not valid for d< 5 nm, therefore, eq 4 should not be valid either. We do not know whether eq 2 and, hence, eq 4 still hold for d> 8.5 Figure 3. (a) Intraband absorption spectra of QDs of different sizes normalized to the peak maxima. (b) Energy of the intraband transition, at RT, as a function of the dot diameter. Data are obtained as the central energies of Gaussian fits of absorption spectra such as those presented in (a). The error bars are estimates of the uncertainty in the fits (±3 meV). The red solid line corresponds to eq 4. The black dashed line represents the energy difference between the second and first excitons. (c) Second confinement energy (E2−Eg) divided by the first confinement energy (E1−Eg) as a function of the first confinement energy. E2 (1Sh−1Pe) is obtained in two ways: directly from absorption spectra at RT (◇) and as EIB (1Se−1Pe)+E1(1Sh−1Se) at RT (●) and 98 K (☆). ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7163 cd conventionally exploited interband transitions and can even be smaller than the band gap of the bulk counterpart, thus allowing exploitation of part of the electromagnetic spectrum forbidden for a given bulk SC material. To give an example of its potential, fine-tuning of and access to intraband transitions in CQDs could lead to photodetectors and light sources in the MWIR and LWIR 11 made of relatively high bandgap, cheap, and nontoxic materials, replacing the current technology based on epitaxially grown HgCdTe, InGaAs and GaInSb. 12 Consequently, work in this field is becoming more and more intense, and steady-state probing of intraband transitions has already been achieved in several materials. 13 However, until recently only mercury chalcogenide CQDs have exhibited stable high doping that allowed fabrication of intraband photodetectors. 11,14,15 Recently, robust heavy doping has been demonstrated in PbS CQD films, 16 enabling intraband absorption and photodetection in the MWIR and LWIR, 17 at energies smaller than the PbS bulk band gap. At this point, studies of the basic properties of intraband transitions in CQDs are needed to guide the development of intrabandbased devices and applications. In this work, we investigate the size and temperature dependence of intraband transitions in the CB of PbS CQDs. We report the intraband absorption coefficient of PbS QD films and discuss the size dependence of the oscillator strength of the first intraband transition in PbS QDs. RESULTS AND DISCUSSION PbS CQDs and Doped Films Used for the Study. Figure 1 shows absorbance spectra of the PbS CQDs used in this study, which evidence good control on the QD size (diameter) in the 5−9 nm range and low size dispersion. QD size has been obtained using the empirical model for oleic-acid capped QDs reported in ref 6after fitting the exciton energy in the absorbance spectra. After synthesis, we fabricated doped films following the method reported in ref 16. The films are spin-coated layer-by- layer on silicon substrates, exchanging the original oleic acid ligand with iodine. We use semi-insulating (lightly doped) silicon substrates throughout the whole study because the different measurements performed require transparency in the 1−12 μm range. After formation, the film is infiltrated and capped with alumina by atomic layer deposition, a method that has been proven to provide n-doping in PbSe 18 and ZnO 19,20 QDs. The resulting PbS CQD films are heavily n-doped (∼ 1019 cm−3) 16 and, consequently, exhibit steady-state intraband absorption in the CB. 17 Figure 2b shows the first two interband excitons in the doped films as a function of the dot diameter, d, obtained via analysis of the absorption spectra, as shown in Figure 2a. Note that for some samples, E2could not be accurately fitted, hence the reduced number of data points for E2in Figure 2b. We found that the first exciton is red-shifted in the doped films as compared to the as-synthesized solutions (Supporting Figure S1). We used this exciton-shift fingerprint as well as the doping level of the samples (discussed later and shown in Figure 4d) to discard oxidation of the dots before or during film formation, thus guaranteeing proper sample quality for further quantitative studies. We found that the samples that showed signs of oxidation (slight blue-shift of the first exciton) also exhibited lower doping levels. We have fitted the first exciton, E1(1Sh−1Se), and the second exciton, E2(1Sh−1Pe), with eqs 1and 2: =+ +Edd (eV) 0.41 1.50 4.2 12(1) with a fit correlation coefficient, R2> 0.99. =+ +Edd (eV) 0.41 3.09 1.4 22 (2) with R2> 0.99. The constant term 0.41 eV is the bulk band gap of PbS, Eg, at room temperature (RT). The size-dependent 1/d2 represents the confinement energy characteristic of particles Figure 1. Absorbance spectra, normalized to the maximum of the exciton peaks, of oleic-acid capped PbS CQDs dispersed in toluene. The QD diameter of the different solutions ranges between 5.2 and 9.0 nm. Figure 2. Interband absorption in heavily n-doped PbS CQD films. (a) Second-derivative analysis of the absorption spectrum. Vertical lines indicate the first three excitons. (b) Energy of the first two excitons, corresponding to lines 1 and 2 in (a) as a function of d. The lines are fits, as described in the main text. The inset illustrates the transitions of the first (red arrow) and second (blue arrows) excitons. Resulting from the n-doped character of the QDs, the measured E2originates exclusively from 1Sh−1Pe transitions and not from 1Ph−1Setransitions. ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7162 conventionally exploited interband transitions and can even be smaller than the band gap of the bulk counterpart, thus allowing exploitation of part of the electromagnetic spectrum forbidden for a given bulk SC material. To give an example of its potential, fine-tuning of and access to intraband transitions in CQDs could lead to photodetectors and light sources in the MWIR and LWIR 11 made of relatively high bandgap, cheap, and nontoxic materials, replacing the current technology based on epitaxially grown HgCdTe, InGaAs and GaInSb. 12 Consequently, work in this field is becoming more and more intense, and steady-state probing of intraband transitions has already been achieved in several materials. 13 However, until recently only mercury chalcogenide CQDs have exhibited stable high doping that allowed fabrication of intraband photodetectors. 11,14,15 Recently, robust heavy doping has been demonstrated in PbS CQD films, 16 enabling intraband absorption and photodetection in the MWIR and LWIR, 17 at energies smaller than the PbS bulk band gap. At this point, studies of the basic properties of intraband transitions in CQDs are needed to guide the development of intrabandbased devices and applications. In this work, we investigate the size and temperature dependence of intraband transitions in the CB of PbS CQDs. We report the intraband absorption coefficient of PbS QD films and discuss the size dependence of the oscillator strength of the first intraband transition in PbS QDs. RESULTS AND DISCUSSION PbS CQDs and Doped Films Used for the Study. Figure 1 shows absorbance spectra of the PbS CQDs used in this study, which evidence good control on the QD size (diameter) in the 5−9 nm range and low size dispersion. QD size has been obtained using the empirical model for oleic-acid capped QDs reported in ref 6after fitting the exciton energy in the absorbance spectra. After synthesis, we fabricated doped films following the method reported in ref 16. The films are spin-coated layer-by- layer on silicon substrates, exchanging the original oleic acid ligand with iodine. We use semi-insulating (lightly doped) silicon substrates throughout the whole study because the different measurements performed require transparency in the 1−12 μm range. After formation, the film is infiltrated and capped with alumina by atomic layer deposition, a method that has been proven to provide n-doping in PbSe 18 and ZnO 19,20 QDs. The resulting PbS CQD films are heavily n-doped (∼ 1019 cm−3) 16 and, consequently, exhibit steady-state intraband absorption in the CB. 17 Figure 2b shows the first two interband excitons in the doped films as a function of the dot diameter, d, obtained via analysis of the absorption spectra, as shown in Figure 2a. Note that for some samples, E2could not be accurately fitted, hence the reduced number of data points for E2in Figure 2b. We found that the first exciton is red-shifted in the doped films as compared to the as-synthesized solutions (Supporting Figure S1). We used this exciton-shift fingerprint as well as the doping level of the samples (discussed later and shown in Figure 4d) to discard oxidation of the dots before or during film formation, thus guaranteeing proper sample quality for further quantitative studies. We found that the samples that showed signs of oxidation (slight blue-shift of the first exciton) also exhibited lower doping levels. We have fitted the first exciton, E1(1Sh−1Se), and the second exciton, E2(1Sh−1Pe), with eqs 1and 2: =+ +Edd (eV) 0.41 1.50 4.2 12(1) with a fit correlation coefficient, R2> 0.99. =+ +Edd (eV) 0.41 3.09 1.4 22 (2) with R2> 0.99. The constant term 0.41 eV is the bulk band gap of PbS, Eg, at room temperature (RT). The size-dependent 1/d2 represents the confinement energy characteristic of particles Figure 1. Absorbance spectra, normalized to the maximum of the exciton peaks, of oleic-acid capped PbS CQDs dispersed in toluene. The QD diameter of the different solutions ranges between 5.2 and 9.0 nm. Figure 2. Interband absorption in heavily n-doped PbS CQD films. (a) Second-derivative analysis of the absorption spectrum. Vertical lines indicate the first three excitons. (b) Energy of the first two excitons, corresponding to lines 1 and 2 in (a) as a function of d. The lines are fits, as described in the main text. The inset illustrates the transitions of the first (red arrow) and second (blue arrows) excitons. Resulting from the n-doped character of the QDs, the measured E2originates exclusively from 1Sh−1Pe transitions and not from 1Ph−1Setransitions. ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7162 a b in a well under the effective mass approximation. The 1/dterm is an empirical observation required to fitE1and E2, as it was the case in previous studies, 6,21 indicating that corrections to this approximation are needed. In both transitions, the 1/d term is dominant over the quantum confinement one, as it is the case in as-synthesized PbS CQDs. 6 In fact, for E2, data can be fitted without the 1/d2term, in the 5 nm < d< 8 nm range, with R2> 0.99. However, the fact that the 1/d2term of E2is almost negligible in this size range is not particular of doped dots. Cademartiri et al. 21 showed that the second exciton in undoped PbS CQDs dispersed in solution deviates from the expected behavior for d> 5 nm, which caused E2to not be fitted to an equation of the form of eq 1 in the 4−7 nm size range. Therefore, although we expect eq 1 to be valid for d<5 nm, 6,21 we do not expect the same for eq 2. There is not a clear explanation for the peculiar size dependence of E2. Although it was a cause of controversy in the past, there is now a consensus that it corresponds to the 1Sh−1Peand 1Ph−1Setransitions. 22,23 These two have very similar energies due to the almost identical electron and hole effective masses in PbS, 24 as indicated in the inset of Figure 2b. Both transitions should be forbidden by symmetry. However, it has been shown that parity selection rules are relaxed in PbS QDs, allowing optical absorption features that do not conserve parity. 22 It has been discussed that breaking of the inversion symmetry of the wave function is needed to fully explain the optical absorption spectra of PbS QDs. 23 Ref 21 shows yet another higher-energy transition (seventh exciton) that exhibits a size dependence behavior similar to E2, with a sudden change in trend for d> 5 nm, and discusses the possibility that this transition originates from a separate corner of the Brillouin zone. Here, we propose another explanation for the sudden change in the size dependence of E2. It has been reported that the morphology of PbS QDs changes with size, evolving from an octahedral shape, for d< 3 nm, to a cuboctahedral shape, for d> 4 nm. 25 Small QDs have Pb-rich (111) facets, whereas in larger dots, S-rich (100) facets emerge. We argue that the change in morphology in large dots, having exposed sulfur atoms, may contribute to the formation of new states that modify the energy of the second (and possibly the seventh) interband transition. Size Dependence of the Intraband Transition. We have measured the absorption spectra of the intraband transitions in our films, Afilm, by means of transmission and reflection measurements via Fourier transform infrared spectroscopy. Our samples consist of a thin film (∼100 nm) of PbS QDs on top of a substrate (∼300 μm) of semi-insulating silicon, as sketched in Supporting Figure S2.Afilm is defined as =−−− A RTA1 film meas meas subs (3) where Rmeas and Tmeas are the measured transmission and reflection, and Asubs is the absorption of the substrate, which was previously characterized through reflection and transmission measurements (see Supporting Figure S3). Figure 3a shows that the intraband transition shifts to higher energies as the dot size decreases, owing to increased quantum confinement. Sharp features at around 0.14 and 0.15 eV arise from the differences (such as the amount of SiO2) in the reference silicon substrate and the substrate of each sample (see Supporting Figure S4). Below 0.13 eV, alumina contributes to absorption (Supporting Figure S5). The size dependence of the intraband energy, EIB, at RT is plotted in Figure 3b. We have fitted the results with eq 4: =−Edd (eV) 1.57 2.5 IB 2(4) with R2= 0.97. The negative value of the 1/d2term is expected, since we expect EIB to be equal to E2−E1(see eqs 1 and 2). For comparison, we have plotted E2−E1in Figure 3b. These results support the fact that, for all studied samples, the absorption peaks analyzed correspond to intraband transitions. As it was the case for E1and E2, the 1/dterm represents the dominant contribution to the size dependence of EIB. This will be useful later on for the analysis of the temperature dependence of EIB.As discussed previously, eq 2 is not valid for d< 5 nm, therefore, eq 4 should not be valid either. We do not know whether eq 2 and, hence, eq 4 still hold for d> 8.5 Figure 3. (a) Intraband absorption spectra of QDs of different sizes normalized to the peak maxima. (b) Energy of the intraband transition, at RT, as a function of the dot diameter. Data are obtained as the central energies of Gaussian fits of absorption spectra such as those presented in (a). The error bars are estimates of the uncertainty in the fits (±3 meV). The red solid line corresponds to eq 4. The black dashed line represents the energy difference between the second and first excitons. (c) Second confinement energy (E2−Eg) divided by the first confinement energy (E1−Eg) as a function of the first confinement energy. E2 (1Sh−1Pe) is obtained in two ways: directly from absorption spectra at RT (◇) and as EIB (1Se−1Pe)+E1(1Sh−1Se) at RT (●) and 98 K (☆). ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7163 in a well under the effective mass approximation. The 1/dterm is an empirical observation required to fitE1and E2, as it was the case in previous studies, 6,21 indicating that corrections to this approximation are needed. In both transitions, the 1/d term is dominant over the quantum confinement one, as it is the case in as-synthesized PbS CQDs. 6 In fact, for E2, data can be fitted without the 1/d2term, in the 5 nm < d< 8 nm range, with R2> 0.99. However, the fact that the 1/d2term of E2is almost negligible in this size range is not particular of doped dots. Cademartiri et al. 21 showed that the second exciton in undoped PbS CQDs dispersed in solution deviates from the expected behavior for d> 5 nm, which caused E2to not be fitted to an equation of the form of eq 1 in the 4−7 nm size range. Therefore, although we expect eq 1 to be valid for d<5 nm, 6,21 we do not expect the same for eq 2. There is not a clear explanation for the peculiar size dependence of E2. Although it was a cause of controversy in the past, there is now a consensus that it corresponds to the 1Sh−1Peand 1Ph−1Setransitions. 22,23 These two have very similar energies due to the almost identical electron and hole effective masses in PbS, 24 as indicated in the inset of Figure 2b. Both transitions should be forbidden by symmetry. However, it has been shown that parity selection rules are relaxed in PbS QDs, allowing optical absorption features that do not conserve parity. 22 It has been discussed that breaking of the inversion symmetry of the wave function is needed to fully explain the optical absorption spectra of PbS QDs. 23 Ref 21 shows yet another higher-energy transition (seventh exciton) that exhibits a size dependence behavior similar to E2, with a sudden change in trend for d> 5 nm, and discusses the possibility that this transition originates from a separate corner of the Brillouin zone. Here, we propose another explanation for the sudden change in the size dependence of E2. It has been reported that the morphology of PbS QDs changes with size, evolving from an octahedral shape, for d< 3 nm, to a cuboctahedral shape, for d> 4 nm. 25 Small QDs have Pb-rich (111) facets, whereas in larger dots, S-rich (100) facets emerge. We argue that the change in morphology in large dots, having exposed sulfur atoms, may contribute to the formation of new states that modify the energy of the second (and possibly the seventh) interband transition. Size Dependence of the Intraband Transition. We have measured the absorption spectra of the intraband transitions in our films, Afilm, by means of transmission and reflection measurements via Fourier transform infrared spectroscopy. Our samples consist of a thin film (∼100 nm) of PbS QDs on top of a substrate (∼300 μm) of semi-insulating silicon, as sketched in Supporting Figure S2.Afilm is defined as =−−− A RTA1 film meas meas subs (3) where Rmeas and Tmeas are the measured transmission and reflection, and Asubs is the absorption of the substrate, which was previously characterized through reflection and transmission measurements (see Supporting Figure S3). Figure 3a shows that the intraband transition shifts to higher energies as the dot size decreases, owing to increased quantum confinement. Sharp features at around 0.14 and 0.15 eV arise from the differences (such as the amount of SiO2) in the reference silicon substrate and the substrate of each sample (see Supporting Figure S4). Below 0.13 eV, alumina contributes to absorption (Supporting Figure S5). The size dependence of the intraband energy, EIB, at RT is plotted in Figure 3b. We have fitted the results with eq 4: =−Edd (eV) 1.57 2.5 IB 2(4) with R2= 0.97. The negative value of the 1/d2term is expected, since we expect EIB to be equal to E2−E1(see eqs 1 and 2). For comparison, we have plotted E2−E1in Figure 3b. These results support the fact that, for all studied samples, the absorption peaks analyzed correspond to intraband transitions. As it was the case for E1and E2, the 1/dterm represents the dominant contribution to the size dependence of EIB. This will be useful later on for the analysis of the temperature dependence of EIB.As discussed previously, eq 2 is not valid for d< 5 nm, therefore, eq 4 should not be valid either. We do not know whether eq 2 and, hence, eq 4 still hold for d> 8.5 Figure 3. (a) Intraband absorption spectra of QDs of different sizes normalized to the peak maxima. (b) Energy of the intraband transition, at RT, as a function of the dot diameter. Data are obtained as the central energies of Gaussian fits of absorption spectra such as those presented in (a). The error bars are estimates of the uncertainty in the fits (±3 meV). The red solid line corresponds to eq 4. The black dashed line represents the energy difference between the second and first excitons. (c) Second confinement energy (E2−Eg) divided by the first confinement energy (E1−Eg) as a function of the first confinement energy. E2 (1Sh−1Pe) is obtained in two ways: directly from absorption spectra at RT (◇) and as EIB (1Se−1Pe)+E1(1Sh−1Se) at RT (●) and 98 K (☆). ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7163 cd
57 𝐸E=0.41+1.50 𝑑+4.2 𝑑C Equation 5.4 𝐸C=0.41+3.09 𝑑+1.4 𝑑C Equation 5.5 In these fits, 0.41 eV is the bulk bandgap of PbS at RT. 1/d2 term represents the confinement energy of particles in a well under the effective mass approximation. 1/d term is an empirical observation required for the fits and used in previous studies as well.55,96 The absorption spectra (Afilm) for the intraband transitions for the dots are shown in Figure 5.6-c. Note that it was not possible to obtain a reliable signal for some of the samples. We have observed that as the dot size increases, intraband transition energy shifts to lower energies as a result of decreased quantum confinement. Sharp dips around 0.14 and 0.15 eV are a result of a combination of native SiO2 and other adsorbents on the Si substrate that vary between the reference and the sample. Intraband transition energies are plotted in Figure 5.6-d as markers with an error of ±3 meV. A fit to the data turns out to be: 𝐸'(&/.J.(* =#1.57 𝑑−2.5 𝑑C Equation 5.6 and is indicated with a red solid line. The black dashed line is the curve E2-E1 and is match quite well the red line. These results support that the absorption peaks analyzed correspond to the intraband transitions for all studied samples. Figure 5.7 – Absorption coefficient ( a ) of the samples. (a) Absorption coefficient spectra for intraband transitions in three films of various sized PbS QDs. (b) Peak values of a for intraband (red markers) and interband (blue markers) calculated from Gaussian fittings to spectral a measurements. Error bars account for the uncertainties in film thickness and noise in absorption measurements. (c) Integrated a , labelled as a , over the energies covered by the Gaussian fits. nm. We know, however, that EIB should get progressively closer to zero as the quantum confinement gets weaker. For dot diameters close to the exciton Bohr radius, aB, of PbS (∼20 nm), the nanocrystals are in the weak confinement regime and EIB should approach zero. In the framework of the effective mass approximation, the normalized confinement energy of the different interband transitions (confinement energy of exciton i,Ei−Eg, divided by the confinement energy of the first exciton, E1−Eg) should be independent of E1−Eg. 10 Figure 3c plots the normalized confinement energy of the second intraband transition. We have used two set of values for E2, those obtained directly from absorption measurements (Figure 2b) and values obtained as E1+EIB (Figures 2b and 3b). As expected, both sets of values yield very similar results. However, instead of a sizeindependent value, we observe a linear decrease of the normalized confinement energy of the second exciton for E1 −Egin the 0.25−0.45 eV range (8 nm > d> 5 nm). This behavior matches the one reported for undoped PbS CQDs dispersed in solution, 21 where (E2−Eg)/(E1−Eg)≈1.39 for E1−Eg> 0.45 eV (d< 5 nm) and increases for smaller confinement energies (larger dots). We ascribe this behavior to the fact that both E1and E2have a predominant 1/d contribution over the 1/d2confinement energy term, as discussed in the previous section. Figure 3c also shows measurements of (E2−Eg)/(E1−Eg) at 98 K. To calculate Egat low temperatures, we used 320 μeV/K as the temperature dependence of the bulk PbS band gap. 26 The low-temperature values of normalized confinement energies match closely the values at RT, indicating that E1and E2at low temperatures follow similar size dependences to those shown in Figure 2b. The impact of temperature on the intraband transition will be studied later on. Absorption Coefficient of Doped PbS QD Films. Characterizing the intrinsic absorption intensity of a semiconductor is crucial both for its use in practical applications and for theoretical studies. We have performed absorption measurements such as those shown in Figure 3a to calculate the absorption coefficient of our films (see Methods). Figure 4a shows some of the measured absorption coefficient spectra of the intraband region. The peak values of αfor the 1Se−1Pe transition are plotted in Figure 4b as a function of d. The α peak values and other relevant parameters of the results presented in Figure 4 are compiled in Supporting Table S1. For comparison, αfor the interband (1Sh−1Se) transition in the same samples is also plotted in Figure 4b. Note that in these absorption measurements, we have not been able to measure the interband transitions for all samples, and the reason is two-fold: For the samples with smaller QDs, the exciton energy falls out of the detector range. For the samples with larger QDs, the interband absorption peak is almost completely bleached (1Sealmost completely filled). The measured interband absorption coefficient in these heavily doped samples is around 0.5 ×104cm−1. From this value, we can estimate what the interband absorption coefficient would be in undoped samples. The interband absorption peak in the doped samples has been bleached to about a quarter of its value prior to doping (Supporting Figure S6). Therefore, the interband absorption coefficient for undoped or lightly doped films would be in the order of 2 ×104cm−1, similar to the measured value of the intraband absorption coefficient and Figure 4. Absorption coefficients in heavily n-doped PbS CQD films. (a) Absorption coefficient spectra measured in PbS QD thin films for QDs of different sizes. (b) Peak values of the intraband (red circles) and interband (blue rhombus) absorption coefficients. Values are obtained by fitting the absorption spectra to Gaussians. The error bars account for the error propagation of the uncertainty in film thickness (see Supporting Table S1) and the absorption measurements (5%, estimated). (c) Integrated absorption coefficients. Values are obtained by integration of the fitted Gaussians. (d) Measured occupancy factor of 1Se. (e) The maximum attainable value of α,αmax, and oscillator strength per volume of the intraband and interband absorption. The line is a power law fit. (f) Oscillator strength per QD of the intraband absorption. ACS Nano www.acsnano.org Article https://dx.doi.org/10.1021/acsnano.0c02033 ACS Nano 2020, 14, 7161−7169 7164 abc
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 58 Figure 5.7 summarizes the absorption coefficients, a, calculated for the same samples as discussed previously in the text. Figure 5.7-a shows three examples of spectral a over the intraband energies. Gaussian fits are performed on this data and in Figure 5.7-b, the intensities of these Gaussians are plotted with respect to QD size with red markers. As a comparison, values for interband transitions of some samples are also plotted in the same figure. It was not possible to obtain interband values for all samples; in some samples the interband signal falls out of the detector range and in the others the bleach in exciton is so severe that a meaningful peak cannot be identified. However, in the samples we have observed, intraband signal intensity was always stronger than interband – an indication of heavy doping and population of the 1Se level. We also calculated the integrated a over the whole Gaussian fit in order to better compare different films with slightly different QD size distributions. These results are shown in Figure 5.7-c indicating a similar behavior as in Figure 5.7-b. Integration over the whole spectrum of the transition corrects for the impact on a peak values of differences in full width half maxima. 5.5 - Occupation of the Conduction Level and Sizedependent Doping In their 1Se state, PbS QDs can accommodate up to 8 electrons due to the eightfold degeneracy in these states including spin.99 It is possible to calculate the number of electrons in the 1Se state by simply measuring the amount of excitonic bleach in our samples. We measure the excitonic absorption by previously mentioned methods before and after alumina deposition, assuming that the doping before alumina deposition is low enough to consider 1Se state non-occupied. We define an occupancy factor for the 1Se state as: ∅=1−𝐼C 𝐼E Equation 5.7 where I1 and I2 are the integrated absorption strength of the excitonic transition of the lightly doped (before alumina) and heavily doped (after alumina) samples respectively. As the size of the PbS QDs increase, a peculiar transition takes place in the surface of the QDs. Smaller-sized QDs up to about 4-5 nm diameter have an octahedral shape with Pb-rich (111) surfaces. As the diameter of the QD increase even further, its morphology starts to evolve into a cuboctahedron with increasing sulfur rich (100) surfaces. As previously explained in this chapter, doping is effective on the (100)
59 surface due to the aliovalent anionic substitution of S-2 with I-. Beygi and coworkers summarized this morphology change in Figure 5.8-a. Figure 5.8 – (a) Evolution of the shape of the PbS QDs and appearance of different surfaces with respect to the diameter of the QDs adapted from 91. Yellow dots indicate sulfur atoms and gray ones are lead atoms. (100) surface emerges as the dot diameter grows above 4-5 nm. (b) Occupancy factor ( f ) versus dot diameter obtained from exciton bleaching measurements. Dotted line is a sigmoid fit to the data. (c) Energy levels for EMII treated films extracted from UPS measurements. Fermi level goes above the conduction band as the dot size increases as a result of higher doping due to a larger sulfur replacement on the (100) surface. In our doped samples, we also observe the effect of the morphology change. In Figure 5.8-b, occupancy factor, f, is plotted against dot diameter. The S-shaped curve is in agreement with the increase in exposed (100) surfaces as the morphology changes. Below a QD diameter of 4 nm, we don’t observe any bleach in the excitonic absorption or an intraband signal due to a lack of (100) surfaces. 4 5 6 7 8 QD Diameter (nm) 0 0.2 0.4 0.6 0.8 1 Occupancy Factor of 1S e ( ) 2 3 4 5 6 7 8 9 QD Diameter (nm) -5.5 -5 -4.5 -4 -3.5 Energy (eV) 1Sh 1Se Ef 1Pe Supplementary data associated with this article can be found, in the online version, at https://doi.org/10.1016/j.apsusc.2018.06.152. 3. Results and discussion 3.1. Size dependent shape and composition of PbS QDs In order to study the surface chemistry of PbS QDs, it is required to investigate the shape of nanoparticles and the corresponding arrangement of Pb and S atoms on their surfaces. The shape of nanoparticles is controlled by the thermodynamics as well as growth kinetic which is affected by the synthesis conditions such as time and temperature as well as type of the capping ligands [21]. According to the Gibbs thermodynamic principle, the equilibrium shape of a nanoparticles is obtained by minimizing the surface energy for a given volume. Wulff construction is a simple method for predicting the thermodynamic equilibrium shape of nanoparticles based on surface energy minimization theorem [29–31]. In this method, the equilibrium shape of particle is that which minimizes ∑A i γ i where A i is the area of the i th plane with the surface energy of γ i . While surface energy of each plane is proportional to the length of a vector drawn normal to a crystal face (γ i =h i ) [29], the Wulffconstruction ratio for specific planes (hkl) can be introduced by equation (1): =γγ(hkl)/ (100) h(hkl)/h(100) (1) According to the calculated surface energies of each planes of specific sized particles, (1 1 1)/(1 0 0) Wulffconstruction ratio calculated for PbS QDs of 1 to 7.5 nm diameter (Table S1). Here, different values of (1 1 1)/(1 0 0) Wulffconstruction ratios represent different equilibrium shape of QDs. While a ratio of 1/√3 corresponds to octahedron morphology, ratios between 1/√3 and 2/√3 are related to truncated octahedron morphology and a ratio of 2/√3 corresponds to a cuboctahedron shape of QDs. Based on the calculated Wulffconstruction ratios, PbS particles smaller than 2.7 nm are octahedrons with eight (1 1 1) surface facets. But with particle size increasing, the particles have truncated (1 0 0) facets to reduce their surface energy and cuboctahedron-shape particles result when the QD sizes exceed 4.74 nm. As well, these model results are in agreement with Bealing’s model concerning PbSe QDs surfaceoleate ligand interactions [21] and Zherebetsky’s model concerning the surface energy of different planes [22]. Together, this indicates that models that predict fully Pb terminated spherical lead chalcogenide QDs [17] cannot be correct. The presented model suggested that the QDs’morphology, surface facets and elemental arrangement on these facets are directly related to the size of QDs. Based on the Wulffconstruction results with respect to the equilibrium shapes of QDs of a given size, we use an atomistic model to “build”the corresponding FCC crystal, which allows us to predict the number and arrangement of Pb and S atoms in the core and on the surface of different sized PbS QDs. The atomistic model results for QDs of 1–7.5 nm diameters are shown in Fig. 1a, and the corresponding atomic counts are reported in Table S1. Fig. 1b shows the arrangement of Pb and S atoms on the surface of typical octahedron and cuboctahedron PbS QDs. The (1 1 1) facets that cover the octahedron particles are completely terminated by Pb atoms. Distinctly, the surface of cuboctahedron particles consists of eight (1 1 1) hexagonal facets and six (1 0 0) square facets. Polar (1 1 1) facets completely terminated by Pb atoms with a coordination number of three, and make up 77.6% of whole surface of the particles. In contrast, nonpolar (1 0 0) facets which make up 22.4% of the particle’s surface, have checkerboard arrangement of Pb and S atoms. Fig. 2a shows the TEM image of typical PbS QDs with mean particle size of 4 nm indicates. According to the HR-TEM images of such particles (Fig. 2b), synthesized QDs have the truncated octahedral morphology, with ordered fringes arrangement representing the preparation of single crystal particles. Based on the Fast Fourier Transform (FFT) pattern presented in Fig. 2c, the two types of planes observed in HR-TEM images (with about interplanar spacing of 2.8 and 3.5 Å) are related to (1 0 0) and (1 1 1) crystalline planes of PbS nanocrystals, respectively. By calculating the length of vectors drawn normal to different crystal faces of HR-TEM images, the (1 1 1)/(1 0 0) facet normal ratios for 4 nm particles was measured to be ∼0.87, in agreement with the truncated octahedron shape predicted by our Wulffconstruction model. A similar analysis of the HR-TEM images of other literature reports confirms this evolution from octahedron to cuboctahedron PbS QDs [22,26]. X-ray diffraction pattern of such nanoparticles (Fig. 2d) also confirms successful synthesis of rock salt PbS QDs. Lattice constant of QDs is calculated 5.922 Å based on X-ray spectrum, same to the value Fig. 1. (a) Equilibrium shape of 1 to 7.5 nm PbS QDs and (b) arrangement of Pb and S atoms at the surface of octahedron and cuboctahedron PbS quantum dots. H. Beygi et al. $SSOLHG6XUIDFH6FLHQFH² a b c
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 60 Doping change as a consequence of morphology also manifests itself in ultraviolet photoelectron spectroscopy (UPS) measurements. We have analyzed various iodide treated films in UPS and the results are plotted in Figure 5.8-c. Due to the inability of UPS to penetrate the uppermost alumina layer, we were not able to measure the alumina covered films but utilized EMII treated films without alumina; however, as UPS is performed under high vacuum, adsorbed water and oxygen inside the film is partially removed during measurements and we were able to observe high n-doping in our films. Fermi level goes above the 1Se level in larger dots but stays within the bandgap for QDs that only has (111) surfaces. The UPS analysis is performed by a 21.22 eV monochromatic Hel UV source and a correction proposed by Miller and coworkers are made in the valence band fits.100 Figure 5.9 – IDS versus VGS curves for various FETs of PbS QDs of different sizes. In all of the samples, n-doping is evident with increasing IDS values as the QD size increases – indicating higher conductivity. Complementing optical measurements, we also characterized the electrical response of the doped QD films by employing them in field-effect transistors (FETs). On doped-Si/SiO2 samples, we have fabricated Au source and drain contacts with varying lateral gaps of 10 µm – 25 µm. In this geometry doped-Si is used to apply the back-gate voltage (VGS) while we measure source-drain current (IDS). On top of these substrates, we have deposited QDs resulting in thicknesses around 50 nm (2 repetitions of layer-by-layer deposition) of different sizes following the doping procedure. We performed electrical measurements using a semiconductor analyzer 8 ݊ ൌ ூವೄబ ವೄబఓௗ௪ Eq. S4.2 where ܫௌ and ܸௌ are, respectively, the values of ܫௌ and ܸௌ at ܸீൌ Ͳ; ݁ is the elementary charge; and ݀ LVWKHWKLFNQHVVRIWKH4'OD\HUZKLFKZHKDYHPHDVXUHGERWKE\SURILORPHWU\ and FIB-SEM. To calculate the number of electrons per dot, ݊ொ, we use the value ߚ ൎ ͲǤͶ ± 15%, where ߚ is the volumetric packing density of our nanoparticles. ݊ொ ൌఊೂವ ఉ Eq. S4.3 where ߛொ ൌͶ͵ ൗ ߨݎொଷ is the volume of a given QD. ݎொሺܧሻ is the QD radius. Figure S4.1 FET transfer characteristic (ܫௌܸீ) of doped PbS dots with different sizes. The length of the channel, ݈, and the value of ܸௌ for each measurement are indicated. All devices exhibit n-type character.
61 with 4-probe connection inside an electrically isolated setup. A summary of the parameters extracted from these measurements can be found in Table 5.1. Table 5.1 – Extracted parameters from the FET measurements of heavily doped PbS QD films Exciton Wavelength (nm) QD Diameter (nm) e- Mobility (cm2V-1s-1) Carrier Density (cm-3) Conductivity (S cm-1) nQD (e- /QD) 1210 4.2 0.27 4.1 x 1018 0.18 ± 15% 0.21 ± 15% 1286 4.5 0.15 8.9 x 1018 0.21 ± 15% 0.6 ± 15% 1402 5.1 0.038 1.1 x 1019 0.07 ± 15% 1.0 ± 15% 1525 5.8 0.085 3.2 x 1019 0.44 ± 15% 4.3 ± 15% 1572 6.1 0.066 3.4 x 1019 0.36 ± 15% 5.4 ± 15% Electrical characterization of the films also confirms high doping in the films with carrier concentrations in the order of 1019 cm-3. As the QD size increases, we see a similar trend as the optical measurements with increased doping in bigger sized dots. A calculation of electrons per dot (nQD) is also introduced as: 𝑛K> =#𝑛γK> 𝛽 Equation 5.8 where n is the carrier concentration extracted from the FET measurements, γK> is the volume of a QD given by 43 M 𝜋𝑟K>L and 𝛽 is the volumetric packing density of our nanoparticles taken as 0.74 ± 15%. Calculated values for nQD can be seen in Table 5.1. 5.6 - High n-doping at Low Temperatures and its Optical Characterization To gain insight into the behavior of high n-doping of PbS QDs and to ultimately use them in photodetectors, we have characterized our films at low temperatures down to 80 K. Low-temperature measurements are performed using the FTIR as previously described in the chapter with an additional temperature controllable Linkam HFS350EV-PB4 stage cooled by liquid nitrogen. The stage is mounted on the FTIR microscope on the sample holder. With ZnSe windows on both sides of the sample
Chapter 5 – Photodetectors Utilizing Intraband Transitions in PbS QDs 68 A summary of the figures of merit can be seen in Table 5.2. We reach detectivities of 8 x 104 Jones at 7.3 µm at 80 K. Correcting by the shadowing factor of the interdigitated electrodes (∼50%) and the reflectivity of the PbS layer would give rise to internal detectivity values on the order of 105 Jones. Figure 5.16 – Photocurrent versus frequency at 80K for both the intraband and interband peak. Curves have been normalized to have a similar response around 60 Hz. The data presented in Table 5.2 is obtained with a chopping frequency of 11 Hz. We also decided to see the effect of frequency on photocurrent to see how fast our photodetectors can respond to modulated light. We both investigated the interband and intraband transitions at high frequencies. Figure 5.16 shows that both the interband and intraband detection are slow with time constants of above 30 ms for intraband and 200 ms for interband. With a novel high-doping process for PbS QDs, we investigated how doping works in different sizes of QDs and at different temperatures. We studied how the doping changes with exposed facets of PbS. We then fabricated photodetectors utilizing the intraband transitions made available by high-doping and reached wavelength regimes that were not possible with PbS QDs. We obtained detectivities of 8 x 104 Jones at 7.3 µm with a PbS film that has a robust doping in ambient, at different temperatures and also robust in time beyond 2 months of testing. These films can be an alternative to current photodetector technology in the MIR and LWIR. 9 Figure S7. (a) Photocurrent at the first and higher energies excitons for the same sample reported in Figure 2d (top panel) of the main manuscript. (b) Photocurrent versus detection frequency at the intraband and exciton energies for the same sample as in (a). The curves have been normalized to have a similar valuel at 60 Hz. The inverse relationship of the photocurrent with frequency down to 30 Hz indicates that the time constant of the photodetection process is > 30 ms and > 200 ms, for the intraband and exciton energies respectively. Figure S8. Scheme of the QD transport model. ܩ, ܩௌ, ܩ are total conductance, conductance through 1Se channels, and conductance through 1Pe channels, respectively. ܧி is the Fermi level (dashed line).
69 Conclusion As we continue to interact with light and incorporate it into our major technologies, demand for high-performance, low-cost, portable photodetectors that can respond to a wide range of wavelengths will continue to rise. In the infrared, with a widevariety of applications that keeps on expanding, research for alternative active materials is going on. The studies presented in this thesis put forward prototypes of photodetectors that respond in the SWIR-NIR-LWIR regime using lead chalcogenide CQDs that can be alternatives to current technologies. PbS and PbSe QDs are efficient in absorbing light; however, due to their poor electrical characteristics, charge extraction is limited. In chapters 3 and 4, we presented hybrid photodetectors with TMDCs and QDs to solve this problem. Research on 2D materials eventually uncovered these layered materials with high conductivity and easy integrability with silicon-based technologies. Owing to their bandgap, they can be used in transistors with high on/off current ratios. We combined few-layers of TMDCs with QD films to form a hybrid detector. Under illumination, photogenerated electrons in the QD layer are transferred to the underlying TMDC layers with the help of a built-in electric field. Electrons can easily be transferred to the contacts of the photodetector with the help of the high-mobility TMDC layers. On top of that, these electrons can circulate many times in the detector circuitry before they recombine with holes in the QD layer resulting in an inherent gain. PbS QD based hybrid photodetectors with WS2 and MoS2 show record detectivities of 1.0x1012 and 2.8x1011 Jones, respectively, at room temperature with their photoresponse reaching up to 2.1 µm. We extended the response of these hybrid photodetectors further into the infrared with PbSe QDs. Proper analysis of the structure and reducing dark currents from the QD layer with oxide-isolated contacts allowed us to have detectivities of 7.7x1010 Jones with response reaching up to 3 µm at room temperature, highest reported to date for QD detectors at these wavelengths.
70 Until recently, optoelectronics using QDs mainly focused on the transitions along the tunable bandgap. As the QD size increases, quantum confinement effects get looser and the bandgap eventually approaches the bulk bandgap of the material. The bulk bandgap of is therefore putting a low-energy limit on the tunability of QDs. In chapter 5, we presented a novel method to overcome the bandgap limit and obtain photoresponse further into the infrared. We presented an air-stable high n-doping method for PbS QDs that is also stable over long periods of time. Iodine-based ligand treatment on the surface of the QDs in combination with a thin layer of Al2O3, results in highly doped QD films. The doping is high enough so that the electrons occupy the 1Se level and transitions with a more energetic 1Pe level are allowed. As the energy difference between these two conduction levels are smaller compared to the bandgap, QD film can absorb photons that are less energetic than the bulk bandgap. This new intraband transition is also tunable with the QD size, providing another degree of freedom to tune the optical response of the film even across MIR and LWIR. Studies of doping versus QD size and temperature are carried out, revealing more about the doping mechanism. Finally, using the high-doped PbS QD films, we realized photodetectors with the longest-wavelength response ever demonstrated for this material. A detectivity of 8x104 Jones is reached at 7.3 µm at 80K. Considering the bandgap of bulk PbS being around 3.7 µm, we reached far beyond this limit using the intraband transitions. Outlook Equipped with various examples of how high-mobility layers can aid in charge transport from light-sensitive and spectrally tunable QDs, we know that hybrid detectors outperform non-hybrid ones. With a careful selection of QD and transport layer considering the resulting band alignments and using techniques like contactisolation, the performance of these devices can be improved. The bottleneck of exfoliating TMDC films for transistors is being challenged by many groups. Large wafer-scale CVD deposition of WS2 monolayers have already been demonstrated with FET mobilities up to 4 cm2V-1s-1.106 And for MoS2, CVD-growth yields to mobilities exceeding 12 cm2V-1s-1.107 As such techniques develop, hybrid TMDC-QD detectors can be fabricated in a scalable manner, leading to tunable, cost-effective and high performance detectors operating without any cooling and they can compete with existing detectors on the market. Enabling intraband transitions in QDs with long term stability paves the way for countless applications in optoelectronics. It offers a new paradigm in engineering the spectral response of QDs and allows us to probe deeper into the infrared. Along with the photodetectors, we also demonstrated stimulated emission utilizing intraband transitions90 paving the way towards intraband QD lasers in the LWIR.
71 Performance of the intraband photodetectors will be improve by engineering the charge-extraction process to realize detectors with higher responsivities. Hybrids with carefully selected charge-blocking layers can decrease dark currents in the detectors, which is one of the issues of having a highly-doped highly-conductive film. With lower dark currents and improved charge transfer, intraband QD photodetectors operating at room temperature are not far from reach.
72 Bibliography (1) Yole Development. Status of CMOS Image Sensor Industry 2021 Report; 2021. (2) Madelung, O. Semiconductors: Data Handbook; Springer Berlin Heidelberg: Berlin, Heidelberg, 2004. https://doi.org/10.1007/978-3-642-18865-7. (3) Hamamatsu. Infrared Photodetectors; 2021. (4) Rogalski, A. Infrared Detectors, Second Edi.; CRC Press, 2011. (5) Sordillo, L. A.; Pu, Y.; Pratavieira, S.; Budansky, Y.; Alfano, R. R. Deep Optical Imaging of Tissue Using the Second and Third Near-Infrared Spectral Windows. J. Biomed. Opt. 2014, 19 (5), 056004. https://doi.org/10.1117/1.JBO.19.5.056004. (6) Rogalski, A. Infrared Detectors: Status and Trends. Prog. Quantum Electron. 2003, 27 (2–3), 59–210. https://doi.org/10.1016/S0079-6727(02)00024-1. (7) Seifert, W.; Carlsson, N.; Johansson, J.; Pistol, M.-E.; Samuelson, L. In Situ Growth of Nano-Structures by Metal-Organic Vapour Phase Epitaxy. J. Cryst. Growth 1997, 170 (1–4), 39–46. https://doi.org/10.1016/S0022-0248(96)00518- 0. (8) Guyot-Sionnest, P. Colloidal Quantum Dots. Comptes Rendus Phys. 2008, 9 (8), 777–787. https://doi.org/10.1016/j.crhy.2008.10.006. (9) Konstantatos, G.; Sargent, E. H. Colloidal Quantum Dot Optoelectronics and Photovoltaics; Cambridge University Press, 2013. (10) Wise, F. W. Lead Salt Quantum Dots: The Limit of Strong Quantum Confinement. Acc. Chem. Res. 2000, 33 (11), 773–780. https://doi.org/10.1021/ar970220q. (11) Konstantatos, G.; Howard, I.; Fischer, A.; Hoogland, S.; Clifford, J.; Klem, E.; Levina, L.; Sargent, E. H. Ultrasensitive Solution-Cast Quantum Dot
73 Photodetectors. Nature 2006, 442 (7099), 180–183. https://doi.org/10.1038/nature04855. (12) Cao, Y.; Stavrinadis, A.; Lasanta, T.; So, D.; Konstantatos, G. The Role of Surface Passivation for Efficient and Photostable PbS Quantum Dot Solar Cells. Nat. Energy 2016, 1 (4), 16035. https://doi.org/10.1038/nenergy.2016.35. (13) Pradhan, S.; Di Stasio, F.; Bi, Y.; Gupta, S.; Christodoulou, S.; Stavrinadis, A.; Konstantatos, G. High-Efficiency Colloidal Quantum Dot Infrared Light-Emitting Diodes via Engineering at the Supra-Nanocrystalline Level. Nat. Nanotechnol. 2019, 14 (1), 72–79. https://doi.org/10.1038/s41565-018-0312-y. (14) Brown, P. R.; Kim, D.; Lunt, R. R.; Zhao, N.; Bawendi, M. G.; Grossman, J. C.; Bulović, V. Energy Level Modification in Lead Sulfide Quantum Dot Thin Films through Ligand Exchange. ACS Nano 2014, 8 (6), 5863–5872. https://doi.org/10.1021/nn500897c. (15) Sahu, A.; Khare, A.; Deng, D. D.; Norris, D. J. Quantum Confinement in Silver Selenide Semiconductor Nanocrystals. Chem. Commun. 2012, 48 (44), 5458. https://doi.org/10.1039/c2cc30539a. (16) Zhu, C.-N.; Jiang, P.; Zhang, Z.-L.; Zhu, D.-L.; Tian, Z.-Q.; Pang, D.-W. Ag 2 Se Quantum Dots with Tunable Emission in the Second Near-Infrared Window. ACS Appl. Mater. Interfaces 2013, 5 (4), 1186–1189. https://doi.org/10.1021/am303110x. (17) Wang, Y.; Ding, G.; Mao, J.-Y.; Zhou, Y.; Han, S.-T. Recent Advances in Synthesis and Application of Perovskite Quantum Dot Based Composites for Photonics, Electronics and Sensors. Sci. Technol. Adv. Mater. 2020, 21 (1), 278–302. https://doi.org/10.1080/14686996.2020.1752115. (18) Kuyanov, P. Quantum Dot Photodetectors; Tong, X., Wu, J., Wang, Z. M., Eds.; Lecture Notes in Nanoscale Science and Technology; Springer International Publishing: Cham, 2021; Vol. 30. https://doi.org/10.1007/978-3-030-74270-6. (19) Richards, P. L. Bolometers for Infrared and Millimeter Waves. J. Appl. Phys. 1994, 76 (1), 1–24. https://doi.org/10.1063/1.357128. (20) Jones, R. C. Performance of Detectors for Visible and Infrared Radiation; Marton, L. B. T.-A. in E. and E. P., Ed.; Academic Press, 1953; Vol. 5, pp 1–96. https://doi.org/https://doi.org/10.1016/S0065-2539(08)60683-6. (21) Dereniak, E. L.; Boreman, G. D. Infrared Detectors and Systems; John Wiley & Sons: New York, NY, 1996. (22) Kruse, P. W. The Photon Detection Process. In Optical and Infrared Detectors; Springer, 1977; pp 5–69. (23) Planck, M. The Theory of Heat Radiation (Translation); 1914.
74 (24) Martyniuk, P.; Rogalski, A. Quantum-Dot Infrared Photodetectors: Status and Outlook. Prog. Quantum Electron. 2008, 32 (3–4), 89–120. https://doi.org/10.1016/j.pquantelec.2008.07.001. (25) Kagan, C. R.; Murray, C. B. Charge Transport in Strongly Coupled Quantum Dot Solids. Nat. Nanotechnol. 2015, 10 (12), 1013–1026. https://doi.org/10.1038/nnano.2015.247. (26) Balazs, D. M.; Bijlsma, K. I.; Fang, H. H.; Dirin, D. N.; Döbeli, M.; Kovalenko, M. V.; Loi, M. A. Stoichiometric Control of the Density of States in PbS Colloidal Quantum Dot Solids. Sci. Adv. 2017, 3 (9), 1–8. https://doi.org/10.1126/sciadv.aao1558. (27) Konstantatos, G.; Badioli, M.; Gaudreau, L.; Osmond, J.; Bernechea, M.; de Arquer, F. P. G.; Gatti, F.; Koppens, F. H. L. Hybrid Graphene–Quantum Dot Phototransistors with Ultrahigh Gain. Nat. Nanotechnol. 2012, 7 (6), 363–368. https://doi.org/10.1038/nnano.2012.60. (28) Wang, Q. H.; Kalantar-Zadeh, K.; Kis, A.; Coleman, J. N.; Strano, M. S. Electronics and Optoelectronics of Two-Dimensional Transition Metal Dichalcogenides. Nat. Nanotechnol. 2012, 7 (11), 699–712. https://doi.org/10.1038/nnano.2012.193. (29) Chhowalla, M.; Shin, H. S.; Eda, G.; Li, L. J.; Loh, K. P.; Zhang, H. The Chemistry of Two-Dimensional Layered Transition Metal Dichalcogenide Nanosheets. Nat. Chem. 2013, 5 (4), 263–275. https://doi.org/10.1038/nchem.1589. (30) Manzeli, S.; Ovchinnikov, D.; Pasquier, D.; Yazyev, O. V; Kis, A. 2D Transition Metal Dichalcogenides. Nat. Rev. Mater. 2017, 2 (8), 17033. https://doi.org/10.1038/natrevmats.2017.33. (31) Kuc, A.; Zibouche, N.; Heine, T. Influence of Quantum Confinement on the Electronic Structure of the Transition Metal Sulfide TS2. Phys. Rev. B - Condens. Matter Mater. Phys. 2011, 83 (24), 1–4. https://doi.org/10.1103/PhysRevB.83.245213. (32) Splendiani, A.; Sun, L.; Zhang, Y.; Li, T.; Kim, J.; Chim, C. Y.; Galli, G.; Wang, F. Emerging Photoluminescence in Monolayer MoS2. Nano Lett. 2010, 10 (4), 1271–1275. https://doi.org/10.1021/nl903868w. (33) Yan, T.; Qiao, X.; Liu, X.; Tan, P.; Zhang, X. Photoluminescence Properties and Exciton Dynamics in Monolayer WSe2. Appl. Phys. Lett. 2014, 105 (10), 101901. https://doi.org/10.1063/1.4895471. (34) Novoselov, K. S.; Jiang, D.; Schedin, F.; Booth, T. J.; Khotkevich, V. V.; Morozov, S. V.; Geim, A. K. Two-Dimensional Atomic Crystals. Proc. Natl. Acad. Sci. 2005, 102 (30), 10451–10453. https://doi.org/10.1073/pnas.0502848102.
75 (35) Fivaz, R.; Mooser, E. Mobility of Charge Carriers in Semiconducting Layer Structures. Phys. Rev. 1967, 163 (3), 743–755. https://doi.org/10.1103/PhysRev.163.743. (36) Kufer, D.; Konstantatos, G. Highly Sensitive, Encapsulated MoS2 Photodetector with Gate Controllable Gain and Speed. Nano Lett. 2015, 15 (11), 7307–7313. https://doi.org/10.1021/acs.nanolett.5b02559. (37) Radisavljevic, B.; Radenovic, A.; Brivio, J.; Giacometti, V.; Kis, A. Single-Layer MoS2 Transistors. Nat. Nanotechnol. 2011, 6 (3), 147–150. https://doi.org/10.1038/nnano.2010.279. (38) Kumar, J.; Kuroda, M. A.; Bellus, M. Z.; Han, S. J.; Chiu, H. Y. Full-Range Electrical Characteristics of WS2 Transistors. Appl. Phys. Lett. 2015, 106 (12). https://doi.org/10.1063/1.4916403. (39) Iqbal, M. W.; Iqbal, M. Z.; Khan, M. F.; Shehzad, M. A.; Seo, Y.; Park, J. H.; Hwang, C.; Eom, J. High-Mobility and Air-Stable Single-Layer WS2 Field-Effect Transistors Sandwiched between Chemical Vapor Deposition-Grown Hexagonal BN Films. Sci. Rep. 2015, 5 (April), 1–9. https://doi.org/10.1038/srep10699. (40) Simsek, E.; Mukherjee, B. Visibility of Atomically-Thin Layered Materials Buried in Silicon Dioxide. Nanotechnology 2015, 26 (45), 455701. https://doi.org/10.1088/0957-4484/26/45/455701. (41) Ottaviano, L.; Palleschi, S.; Perrozzi, F.; D’Olimpio, G.; Priante, F.; Donarelli, M.; Benassi, P.; Nardone, M.; Gonchigsuren, M.; Gombosuren, M.; Lucia, A.; Moccia, G.; Cacioppo, O. A. Mechanical Exfoliation and Layer Number Identification of MoS2 Revisited. 2D Mater. 2017, 4 (4), 045013. https://doi.org/10.1088/2053-1583/aa8764. (42) Coleman, J. N.; Lotya, M.; O’Neill, A.; Bergin, S. D.; King, P. J.; Khan, U.; Young, K.; Gaucher, A.; De, S.; Smith, R. J.; Shvets, I. V.; Arora, S. K.; Stanton, G.; Kim, H. Y.; Lee, K.; Kim, G. T.; Duesberg, G. S.; Hallam, T.; Boland, J. J.; Wang, J. J.; Donegan, J. F.; Grunlan, J. C.; Moriarty, G.; Shmeliov, A.; Nicholls, R. J.; Perkins, J. M.; Grieveson, E. M.; Theuwissen, K.; McComb, D. W.; Nellist, P. D.; Nicolosi, V. Two-Dimensional Nanosheets Produced by Liquid Exfoliation of Layered Materials. Science (80-. ). 2011, 331 (6017), 568–571. https://doi.org/10.1126/science.1194975. (43) Eda, G.; Yamaguchi, H.; Voiry, D.; Fujita, T.; Chen, M.; Chhowalla, M. Photoluminescence from Chemically Exfoliated MoS 2. Nano Lett. 2011, 11 (12), 5111–5116. https://doi.org/10.1021/nl201874w. (44) Lee, Y. H.; Zhang, X. Q.; Zhang, W.; Chang, M. T.; Lin, C. Te; Chang, K. Di; Yu, Y. C.; Wang, J. T. W.; Chang, C. S.; Li, L. J.; Lin, T. W. Synthesis of Large-Area MoS2 Atomic Layers with Chemical Vapor Deposition. Adv. Mater. 2012, 24 (17), 2320–2325. https://doi.org/10.1002/adma.201104798.
76 (45) Yoon, Y.; Ganapathi, K.; Salahuddin, S. How Good Can Monolayer MoS2 Transistors Be? Nano Lett. 2011, 11 (9), 3768–3773. https://doi.org/10.1021/nl2018178. (46) Hu, C.; Dong, D.; Yang, X.; Qiao, K.; Yang, D.; Deng, H.; Yuan, S.; Khan, J.; Lan, Y.; Song, H.; Tang, J. Synergistic Effect of Hybrid PbS Quantum Dots/2D- WSe2 Toward High Performance and Broadband Phototransistors. Adv. Funct. Mater. 2017, 27 (2). https://doi.org/10.1002/adfm.201603605. (47) Kufer, D.; Lasanta, T.; Bernechea, M.; Koppens, F. H. L.; Konstantatos, G. Interface Engineering in Hybrid Quantum Dot–2D Phototransistors. ACS Photonics 2016, 3 (7), 1324–1330. https://doi.org/10.1021/acsphotonics.6b00299. (48) Kufer, D.; Nikitskiy, I.; Lasanta, T.; Navickaite, G.; Koppens, F. H. L.; Konstantatos, G. Hybrid 2D-0D MoS 2 -PbS Quantum Dot Photodetectors. Adv. Mater. 2015, 27 (1), 176–180. https://doi.org/10.1002/adma.201402471. (49) Yu, Y.; Zhang, Y.; Song, X.; Zhang, H.; Cao, M.; Che, Y.; Dai, H.; Yang, J.; Zhang, H.; Yao, J. PbS-Decorated WS2 Phototransistors with Fast Response. ACS Photonics 2017, 4 (4), 950–956. https://doi.org/10.1021/acsphotonics.6b01049. (50) Huo, N.; Gupta, S.; Konstantatos, G. MoS2 -HgTe Quantum Dot Hybrid Photodetectors beyond 2 Μm. Adv. Mater. 2017, 29 (17), 1606576. https://doi.org/10.1002/adma.201606576. (51) Sharma, D.; Motayed, A.; Shah, P. B.; Amani, M.; Georgieva, M.; Glen Birdwell, A.; Dubey, M.; Li, Q.; Davydov, A. V. Transfer Characteristics and Low- Frequency Noise in Single- and Multi-Layer MoS2field-Effect Transistors. Appl. Phys. Lett. 2015, 107 (16), 1–6. https://doi.org/10.1063/1.4932945. (52) Li, H.; Zhang, Q.; Yap, C. C. R.; Tay, B. K.; Edwin, T. H. T.; Olivier, A.; Baillargeat, D. From Bulk to Monolayer MoS 2: Evolution of Raman Scattering. Adv. Funct. Mater. 2012, 22 (7), 1385–1390. https://doi.org/10.1002/adfm.201102111. (53) Qiao, S.; Yang, H.; Bai, Z.; Peng, G.; Zhang, X. Identifying the Number of WS2 Layers via Raman and Photoluminescence Spectrum. In Proc. of the 2017 5th Int. Conf. on Mechatronics, Materials, Chemistry and Computer Engineering (ICMMCCE 2017); 2017. (54) Lee, J. W.; Kim, D. Y.; Baek, S.; Yu, H.; So, F. Photodetectors: Inorganic UV- Visible-SWIR Broadband Photodetector Based on Monodisperse PbS Nanocrystals. Small 2016, 12 (10), 1246–1246. https://doi.org/10.1002/smll.201670050. (55) Moreels, I.; Lambert, K.; Smeets, D.; De Muynck, D.; Nollet, T.; Martins, J. C.; Vanhaecke, F.; Vantomme, A.; Delerue, C.; Allan, G.; Hens, Z. Size-Dependent
77 Optical Properties of Colloidal PbS Quantum Dots. ACS Nano 2009, 3 (10), 3023–3030. https://doi.org/10.1021/nn900863a. (56) Bi, Y.; Bertran, A.; Gupta, S.; Ramiro, I.; Pradhan, S.; Christodoulou, S.; Majji, S.-N.; Akgul, M. Z.; Konstantatos, G. Solution Processed Infrared- and Thermo- Photovoltaics Based on 0.7 EV Bandgap PbS Colloidal Quantum Dots. Nanoscale 2019, 11 (3), 838–843. https://doi.org/10.1039/C8NR08755E. (57) Pradhan, S.; Stavrinadis, A.; Gupta, S.; Bi, Y.; Di Stasio, F.; Konstantatos, G. Trap-State Suppression and Improved Charge Transport in PbS Quantum Dot Solar Cells with Synergistic Mixed-Ligand Treatments. Small 2017, 13 (21), 1700598. https://doi.org/10.1002/smll.201700598. (58) Sim, D. M.; Kim, M.; Yim, S.; Choi, M. J.; Choi, J.; Yoo, S.; Jung, Y. S. Controlled Doping of Vacancy-Containing Few-Layer MoS2 via Highly Stable Thiol-Based Molecular Chemisorption. ACS Nano 2015, 9 (12), 12115–12123. https://doi.org/10.1021/acsnano.5b05173. (59) Liu, S.; Yuan, K.; Xu, X.; Yin, R.; Lin, D. Y.; Li, Y.; Watanabe, K.; Taniguchi, T.; Meng, Y.; Dai, L.; Ye, Y. Hysteresis-Free Hexagonal Boron Nitride Encapsulated 2D Semiconductor Transistors, NMOS and CMOS Inverters. Adv. Electron. Mater. 2019, 5 (2), 2–7. https://doi.org/10.1002/aelm.201800419. (60) Wang, J.; Rhodes, D.; Feng, S.; Nguyen, M. A. T.; Watanabe, K.; Taniguchi, T.; Mallouk, T. E.; Terrones, M.; Balicas, L.; Zhu, J. Gate-Modulated Conductance of Few-Layer WSe2 Field-Effect Transistors in the Subgap Regime: Schottky Barrier Transistor and Subgap Impurity States. Appl. Phys. Lett. 2015, 106 (15). https://doi.org/10.1063/1.4918282. (61) Li, M.; Chen, J. S.; Routh, P. K.; Zahl, P.; Nam, C. Y.; Cotlet, M. Distinct Optoelectronic Signatures for Charge Transfer and Energy Transfer in Quantum Dot–MoS2 Hybrid Photodetectors Revealed by Photocurrent Imaging Microscopy. Adv. Funct. Mater. 2018, 28 (29), 1–9. https://doi.org/10.1002/adfm.201707558. (62) Chiu, M. H.; Tseng, W. H.; Tang, H. L.; Chang, Y. H.; Chen, C. H.; Hsu, W. T.; Chang, W. H.; Wu, C. I.; Li, L. J. Band Alignment of 2D Transition Metal Dichalcogenide Heterojunctions. Adv. Funct. Mater. 2017, 27 (19). https://doi.org/10.1002/adfm.201603756. (63) Kozawa, D.; Carvalho, A.; Verzhbitskiy, I.; Giustiniano, F.; Miyauchi, Y.; Mouri, S.; Castro Neto, A. H.; Matsuda, K.; Eda, G. Evidence for Fast Interlayer Energy Transfer in MoSe2/WS2 Heterostructures. Nano Lett. 2016, 16 (7), 4087–4093. https://doi.org/10.1021/acs.nanolett.6b00801. (64) Mak, K. F.; Lee, C.; Hone, J.; Shan, J.; Heinz, T. F. Atomically Thin MoS2: A New Direct-Gap Semiconductor. Phys. Rev. Lett. 2010, 105 (13), 2–5. https://doi.org/10.1103/PhysRevLett.105.136805.