Full text
TESIS DOCTORAL DESIGN AND STUDY OF MULTIFUNCTIONAL SYSTEMS BASED ON MAGNETIC NANOPARTICLES FOR BIOMEDICAL APPLICATIONS Noelia Guldris Pensado PROGRAMA DE DOCTORADO EN NANOMEDICINA Facultad de Física SANTIAGO DE COMPOSTELA 2017
TESIS DOCTORAL DESIGN AND STUDY OF MULTIFUNCTIONAL SYSTEMS BASED ON MAGNETIC NANOPARTICLES FOR BIOMEDICAL APPLICATIONS Noelia Guldris Pensado DEPARTAMENTO DE FÍSICA APLICADA PROGRAMA DE DOCTORADO EN NANOMEDICINA Facultad de Física SANTIAGO DE COMPOSTELA 2017
José Rivas Rey, Catedrático del Departamento de Física Aplicada de la Universidad de Santiago de Compostela, como director y tutor de esta tesis, y Manuel Bañobre y Laura Salonen investigadores del International Iberian Nanotechnology Laboratory (INL), Braga, (Portugal), como directores de esta tesis: CERTIFICAN que el trabajo titulado “DESIGN AND STUDY OF MULTIFUNCTIONAL SYSTEMS BASED ON MAGNETIC NANOPARTICLES FOR BIOMEDICAL APPLICATIONS” realizado por Noelia Guldris Pensado, ha sido revisado y reúne todos los requisitos exigidos en el artículo 34 del reglamento de los Estudios de Doctorado, y que como no incurre en las causas de abstención establecidas en la ley 30/1992, autorizan su presentación para optar al título de Doctora en la Universidad de Santiago de Compostela por el Programa de Doctorado en Nanomedicina. Santiago de Compostela, 25 Enero 2017 José Rivas Rey Manuel Bañobre López Laura Salonen Director y Tutor Director Directora
This Ph.D. thesis has been carried out at the International Iberian Nanotechnology Laboratory (INL) in collaboration with the University of Santiago de Compostela (USC). The work was funded by POCTEP (Operational Program for Cross-border Cooperation Spain-Portugal) through the ‘InveNNta’ project, a joint initiative between the INL and the Health Research Institute of Santiago de Compostela (IDIS), managed through the Ramón Domínguez Foundation, and co-financed by the ERDF (European Regional Development Fund), by the P.O. Norte CCDR-N/ON.2 program, and by GAIN, Xunta de Galicia.
‘I declare after all there is no enjoyment like reading! How much sooner one tires of any thing than of a book! When I have a house of my own, I shall be miserable if I have not an excellent library.’ Caroline Bingley, Pride and Prejudice
SUMMARY Nanomedicine is a new field employing nanotechnology tools for biomedical applications. Nanomaterials feature sizes between 1 and 100 hundred nanometers, and therefore they fill the gap between single molecules and bulk materials. They open the possibility to access biological processes on the same size scale. Nanoparticles have shown great potential to achieve the goal of personalized medicine due to the possibilities to modify their surface with proteins, targeting molecules, or imaging probes. Particularly, iron oxide nanoparticles show promising properties for successful application in biomedicine due to their low-cost production, high biocompatibility, and great magnetic response. Strategies for the functionalization of inorganic cores have been developed over the past years, and efforts have been devoted to engineering nanoparticles with multifunctional ligands on the surface to enable active tumor targeting, detection over different imaging modalities, and stimulus-driven cargo release. During this Ph.D. thesis, three main aspects of iron oxide nanoparticles have been evaluated. First, the stability of nanoparticles has been addressed in biological fluids. Second, the uptake of nanoparticles by stem cells for cell tracking applications was studied with nanoparticles of different sizes and bearing different organic coatings. Third, new possibilities of chemical functionalization of naked iron oxide nanoparticles by orthogonal processes have been explored, in order to achieve high yields, simplicity and high reproducibility. KEYWORDS: nanoparticles, iron oxide, MRI, cell tracking, click chemistry, DielsAlder, CuAAC, hyperthermia. RESUMEN (ESPAÑOL) La nanomedicina es una nueva área de conocimiento que utiliza las herramientas de la nanotecnología para aplicaciones biomédicas. Los materiales nanoestructurados con tamaños de 1 a 100 nm se encuentran en el rango intermedio entre las pequeñas moléculas y los materiales macroscópicos, y por tanto, ofrecen la posibilidad de interaccionar con procesos biológicos en la misma escala. Las nanopartículas poseen características prometedoras para lograr la ‘medicina personalizada’, gracias a la posibilidad de modificar su superficie con moléculas de interés biológico, como proteínas, ligandos receptores, o sondas de imagen. Las nanopartículas compuestas por óxidos de hierro son particularmente prometedoras por poseer buena respuesta magnética, excelente biocompatibilidad, y bajos costes de producción. En los últimos años se han desarrollado nuevas estrategias para la modificación de nanopartículas de óxidos de hierro, intentando diseñar nanopartículas con propiedades diana que se dirijan a tumores, que además sean detectables mediante varias técnicas de imagen, y que adicionalmente consigan liberar un fármaco mediante estímulos externos. En esta tesis de doctorado se han evaluado tres aspectos fundamentales de nanopartículas de óxidos de hierro para su aplicación en biomedicina. Primero, se ha estudiado el proceso de síntesis y de purificación de nanopartículas de óxido de hierro, así como su interacción con biomoléculas. Segundo, se ha evaluado las diferencias en
internalización en células madre de nanopartículas de óxidos de hierro con varios recubrimientos orgánicos. Tercero, se han explorado nuevos métodos de funcionalización de nanopartículas mediante química ‘click’ que ofrece ventajas como simplicidad, altos rendimientos, y buena reproducibilidad. PALABRAS CLAVE: nanopartículas, óxidos de hierro, MRI, seguimiento de células madre, química click, DielsAlder, CuAAC, hipertermia. RESUMO (GALEGO) A nanomedicina é unha nova área de coñecemento que emprega as ferramentas da nanotecnoloxía para aplicacións biomédicas. Os materiais nanoestruturados con tamaños de 1 a 100 nanómetros encóntranse no rango intermedio entre as pequenas moléculas e os materiais macroscópicos, e polo tanto, ofrecen a posibilidade de interaccionar con procesos biolóxicos na mesma escala. As nanopartículas posúen características prometedoras para lograr a ‘medicina personalizada’, grazas á posibilidade de modificar a súa superficie con moléculas de interese biolóxico, como proteínas, ligandos receptores, ou sondas de imaxe. As nanopartículas compostas por óxidos de ferro son particularmente prometedoras por posuír excelente biocompatibilidade, baixos custos de produción, e resposta magnética. Novas estratexias para a modificación de nanopartículas de óxidos de ferro desenvolvéronse nos últimos anos, tentando deseñar nanopartículas con propiedades diana en tumores, detectables mediante varias técnicas de imaxe, e tamén para externamente inducir á liberación dun fármaco. Nesta tese de doutoramento evaluáronse tres aspectos fundamentais de nanopartículas de óxidos de ferro para a sua aplicación en biomedicina. Primeiro, estudouse o proceso de síntese e de purificación de nanopartículas de óxido de ferro, así como a súa interacción con biomoléculas. Segundo, evaluáronse as diferenzas en internalización en células nai de nanopartículas de óxidos de ferro con diferentes recubrimentos orgánicos. Terceiro, exploráronse novos métodos de funcionalización de nanopartículas mediante química ‘click‘ que ofrece vantaxes como simplicidade, altos rendementos, e alta reproducibilidade. PALABRAS CHAVE: nanopartículas, óxidos de ferro, MRI, cell tracking, química click, DielsAlder, CuAAC, hipertermia.
1 TABLE OF CONTENTS ABBREVIATIONS ........................................................................................................................................................ 5 CHAPTER 1 ................................................................................................................................................................... 9 1 Introduction ........................................................................................................................................................ 9 1.1 Nanomedicine......................................................................................................................................... 10 1.2 Magnetic Nanoparticles ...................................................................................................................... 11 1.2.1 Synthesis Method ........................................................................................................................ 12 1.2.2 Surface Functionalization ........................................................................................................ 14 1.2.3 NP Functionalization: Click Chemistry ............................................................................... 18 1.2.4 1,3-Dipolar Cycloaddition ........................................................................................................ 20 1.2.5 DielsAlder Reaction ................................................................................................................. 21 1.3 Biomedical Applications .................................................................................................................... 24 1.3.1 MRI: T1, T2, and Dual Contrast Agents ................................................................................. 24 1.3.2 Cell Tracking .................................................................................................................................. 28 1.3.3 Labeling Procedures .................................................................................................................. 28 1.3.4 Limitations of IONs for Cell Tracking .................................................................................. 30 1.3.5 Hyperthermia ................................................................................................................................ 31 1.3.6 Magnetic Hyperthermia ............................................................................................................ 32 1.3.7 Drug Delivery ................................................................................................................................ 36 1.3.8 Magnetic Nanohybrids .............................................................................................................. 36 1.3.9 Drug Loading ................................................................................................................................. 37 1.3.10 IONs in the Clinic ......................................................................................................................... 44 1.4 Biointerface ............................................................................................................................................. 45 1.4.1 Protein Corona ............................................................................................................................. 46 1.4.2 Uptake by Cells ............................................................................................................................. 48 CHAPTER 2 ................................................................................................................................................................. 53
2 2 Ultrasmall Magnetic Nanoparticles: MRI performance and in vitro stability ........................ 53 2.1 Introduction ............................................................................................................................................ 54 2.2 Synthesis of IONs .................................................................................................................................. 55 2.3 USPIO Stability ....................................................................................................................................... 63 2.3.1 Chemical Stability ........................................................................................................................ 63 2.3.2 USPIOs Protein Adsorption ..................................................................................................... 65 2.3.3 In vitro Studies .............................................................................................................................. 66 2.4 MRI Measurements .............................................................................................................................. 68 2.5 Conclusions.............................................................................................................................................. 72 2.6 Experimental .......................................................................................................................................... 73 2.6.1 Chemicals ........................................................................................................................................ 73 2.6.2 USPIOs Synthesis Procedure .................................................................................................. 73 2.6.3 Characterization .......................................................................................................................... 74 2.6.4 Nanoparticle Functionalization ............................................................................................. 75 2.6.5 Chemical Stability ........................................................................................................................ 76 2.6.6 USPIO Stability in Biological Medium ................................................................................. 76 2.6.7 Viability Assay .............................................................................................................................. 77 2.6.8 Cell Count ........................................................................................................................................ 77 2.6.9 MRI Measurements ..................................................................................................................... 77 CHAPTER 3 ................................................................................................................................................................. 79 3 Magnetite Nanoparticles for Stem Cell Labeling ............................................................................... 79 3.1 Introduction ............................................................................................................................................ 80 3.2 Synthesis of IONs .................................................................................................................................. 81 3.3 Coating Modification............................................................................................................................ 84 3.4 Fe Content in MSCs ............................................................................................................................... 87 3.5 Cell Health ................................................................................................................................................ 90 3.6 In vivo Studies ......................................................................................................................................... 91
3 3.7 Conclusions.............................................................................................................................................. 94 3.8 Experimental .......................................................................................................................................... 95 3.8.1 Materials and Methods .............................................................................................................. 95 3.8.2 IONs Synthesis Procedure ....................................................................................................... 97 3.8.3 Glucosamine Modification ....................................................................................................... 97 3.8.4 In vitro Experiments ................................................................................................................... 98 3.8.5 Incubation between PLL and USPIO-PAA-GlcN .............................................................. 98 3.8.6 ICP of Labeled MSC ..................................................................................................................... 99 3.8.7 PB Staining ..................................................................................................................................... 99 3.8.8 LDH Assay ....................................................................................................................................... 99 3.8.9 Cell Count ........................................................................................................................................ 99 3.8.10 In vivo Experiments ................................................................................................................. 100 3.8.11 MRI Studies ................................................................................................................................. 100 3.8.12 Agar Phantoms .......................................................................................................................... 100 3.8.13 In vivo MRI ................................................................................................................................... 101 CHAPTER 4 .............................................................................................................................................................. 103 4 Clickable Iron Oxide Nanoparticles ...................................................................................................... 103 4.1 Introduction ......................................................................................................................................... 104 4.2 Allyl-Functionalized IONs ............................................................................................................... 105 4.3 Naked ION Synthesis ........................................................................................................................ 108 4.4 Isocyanates for ION Functionalization ...................................................................................... 110 4.4.1 Synthesis of Isocyanate Ligands ......................................................................................... 110 4.4.2 ION Functionalization with Isocyanates ......................................................................... 112 4.4.3 Model Reactions ........................................................................................................................ 119 4.5 Click Reactions on the NP Surface ............................................................................................... 122 4.6 Conclusions........................................................................................................................................... 131 4.7 Experimental ....................................................................................................................................... 133
4 4.7.1 Synthetic Procedures .............................................................................................................. 135 CHAPTER 5 .............................................................................................................................................................. 155 5 General Conclusions ................................................................................................................................... 155 6 Bibliography .................................................................................................................................................. 159
5 ABBREVIATIONS Abs absorbance Ac2O acetic anhydride AMF alternating magnetic field Aq aqueous BCA bicinchoninic acid BSA bovine serum album CA contrast agent calcd calculated CC column chromatography CPMG Carr Purcell Meiboom Gill CuAAC Cu(I)-catalyzed azidealkyne cycloaddition Cy3-NH2 cyanine3 amine d days DBU 8-diazabicyclo[5.4.0]undec-7-ene Dh hydrodynamic diameter DLS dynamic light scattering DMA N,N-dimethylacetamide DMF N,N-dimethylformamide doxo doxorubicin EDC 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide EDG electron-donating groups EDX energy-dispersive X-ray spectroscopy
6 EGFR epidermal growth factor receptor EI electron impact ionization ESI electrospray ionization eq equivalent EtOAc ethyl acetate EtOH ethanol EWG electron-withdrawing groups FA flip angle FDA food and drug administration FOV field of view FSE fast spin echo FT-IR Fourier transform infrared spectroscopy GlcN D-glucosamine h hours HAADF high-angle annular dark-field Hc coercive force HPF heparin-protamine-Ferumoxytol ICP-OES inductively coupled plasma optical emission spectroscopy IMDM Iscove's Modified Dulbecco's Medium ION iron oxide nanoparticle IR infrared LDH lactate dehydrogenase MeCN acetonitrile MEG multi-gradient echo
7 MEMS multi-echo-multi-sliced MeOH methanol MH magnetic hyperthermia min minutes MRI magnetic resonance imaging MS mass spectrometry Ms saturation magnetization MSC mesenchymal stem cell MSME multi-slice multi-spin-echo sequence MW molecular weight NaOAc sodium acetate NMR nuclear magnetic resonance NP nanoparticle OPA o-phthalaldehyde PAA polyacrylic acid PEG polyethylene glycol PB Prussian blue PBS phosphate buffer saline PC protein corona PI polydispersity index PLA polylactic acid PLL poly-lysine PMMA poly(methyl methacrylate) PTFE poly(tetrafluoroethylene)
Chapter 1 Introduction 14 that stabilizes the isotropic dispersion.7 In particular, water-in-oil microemulsions are the most used to synthesize magnetic NPs, in which the microdroplets act as small nanoreactors. This method offers a relatively good control of the core size and morphology by modifying the organic/aqueous ratio of the solvent mixture.19 However, the yield of the reaction is the lowest compared to the aforementioned methods. Figure 1: A) Experimental set up for thermal decomposition synthesis of IONs, B) Picture of autoclave reactor for hydrothermal synthesis and scheme of the liquid-solid-solution phases, C) Reaction between microdroplets showing the material transfer in order to obtain IONs by microemulsion method. Each of the methods presented above display advantages and disadvantages. The current challenge in NP synthesis20 is the scale-up to obtain NPs with high crystallinity, size monodispersity, controlled morphology, and reproducible organic coverage content. The production of NPs with desirable properties on a high scale is still a milestone that prevents the advance of magnetic NPs for biomedical applications. 1.2.2 Surface Functionalization The surface of naked IONs is composed of Fe and O atoms, where Fe act as a Lewis acid and coordinates water molecules in an aqueous medium.21,22 Therefore, the surface charge, or potential, in naked IONs is pH-dependent: at basic pH it is negative, at acidic pH positive, and at a neutral pH around zero.
Chapter 1 Introduction 15 The prevention of agglomeration of IONs in aqueous medium can be accomplished by steric and/or electrostatic stabilization.23 On one hand, the steric stabilization is adequate to stabilize NPs in solutions with high salt concentration and in a wide range of pH. The strategy relies on the use of polymer shells that maintain the NPs apart due to an increase in the entropy of the polymers when they approach. On the other hand, the electrostatic stabilization relies on the electrostatic repulsion between the NPs, and is thus highly dependent on the salt concentration and pH. The force of electrostatic repulsion can become greater than van der Waals attraction forces when NPs are charged, and lead to stabilization of individual NPs. Both stabilization modes can play a role at the same time in the colloidal stability of the NPs. Therefore, either organic or inorganic coating of IONs is needed for them to be stable at physiological pH,23 to enhance chemical stability, to reduce cytotoxicity, and to confer antifouling properties against biomolecules.8 There are two main approaches to functionalize IONs: in situ functionalization and post-synthesis surface modification.23 In situ functionalization refers to a one-pot synthesis of the inorganic core and the shell at the same time. In this procedure, the chemicals are added together to the reaction mixture. This strategy is simple and time-efficient. Post-synthesis surface modification implies a two-step procedure: first, the inorganic core is synthesized, and second, the addition of molecules with binding affinities to the inorganic core is performed. This strategy offers versatility as there is a broad commercially available catalogue of chelating molecules. Within post-synthesis protocols, the chemical surface modification of IONs can be achieved by ligand addition, ligand exchange, or encapsulation.24 The ligand addition consists of adding the ligand of interest to the prepared NPs, with no removal of other ligands. Contrarily, ligand exchange usually implies the substitution of hydrophobic ligands with hydrophilic ones governed by equilibrium reactions. Third, the IONs can be also efficiently encapsulated in a polymer matrix with hydrophilic/hydrophobic properties. All these functionalization strategies result in different structures and morphological conformations, such as core-shell, mosaic, shell-core, matrix disperse, and shell-core-shell structures (Figure 2).23
Chapter 1 Introduction 16 Figure 2: Structure of core-shell, mosaic, shell-core, and shella-core-shellb NPs. As mentioned, a vast variety of materials also exists for the coating of IONs (Table 1).25 The materials can be classified into two main categories by the nature of their composition: inorganic and organic compounds. Different coating materials affect the colloidal stability, adsorption of molecules, chemical degradability, and magnetic properties of the synthesized NPs. Therefore, the selection of coating must be done bearing in mind the future application of the IONs. Table 1: Classification of materials for surface modification of IONs. Inorganic compounds Organic compounds Silica Small molecules: silanes citrates, phosphates Metals: gold, rare-earth elements Polymers: natural and synthetic Metal oxides: zinc, cobalt ferrites Macromolecules: liposomes, dendrimers One of the most used inorganic coating for IONs is silica, since it gives high colloidal stability, excellent water dispersion, and protection against photodegradation and oxidation.26 The most common methodology uses the Stöber process,27 i.e. the condensation at basic pH of hydroxylic groups at ION surface with orthosilicates. The thickness of the silica layer can be controlled through reaction conditions such as time, pH, or amount of catalyst. The functionalization of the silica coating involves straightforward and well-known chemistry, which gives access to IONs with functional moieties for further attachment of drugs, antibodies, or imaging probes. On the other hand, gold is among the most used metals as coating for IONs due to its ability to be post-functionalized through thiol-gold chemistry.23 Moreover, gold offers a protective layer with relatively low reactivity or chemical inertness. There are
Chapter 1 Introduction 17 several examples in the literature for Au-coated IONs. For example, Sun and coworkers28 reported a method in which HAuCl4 seeds were reduced on the surface of IONs, yielding core-shell nanostructured Au-coated magnetite NPs and preserving the orignal magnetic properties of IONs. However, when transition metal oxides are used as coating, the magnetic properties may change depending on the magnetic nature of the metal oxides phase formed.29 For example, Cheon and coworkers30 reported a heterostructure composed of a core of Fe3O4 coated with cobalt ferrite shell with higher Ms and coercive forces. The main concerns about inorganic coatings are their degradability and toxicity, as opposed to organic materials.23,31 Organic molecules that are able to interact with the IONs’ surface can be divided into small molecules, polymers, and macromolecules (Table 1). Unlike polymers, small molecules are able to enhance the colloidal stability of IONs with little to no increase in the hydrodynamic diameter.23 This characteristic is important when IONs are designed to diffuse to the extravascular space, as particle size plays a fundamental role in NP biodistribution.24 There are several functional groups with high affinity to anchor to the surface of IONs: carboxylates, phosphonates, aminosilanes, and alcohols are the most commonly used.23,26,32 Ligands with multiple functional groups are especially interesting because they interact through multiple bonds.33 Examples of molecules with multiple functional groups are citric acid,34 dimercaptosuccinic acids,35 and dopamine (Figure 3).36 Figure 3: Examples of small molecules for the functionalization of IONs. Oppositely, polymers offer a shell protection with the consequent increase in hydrodynamic diameter. Polymers used in NP coating can be of natural or synthetic nature. Dextran and chitosan are natural polymers based on polysaccharides often used as coating agents due to their high biocompatibility. The large amount of hydroxyl groups in these polymers enables multiple effective interactions by hydrogen bonding between the polymers and the IONs leading to stable nanocolloids.23 For example,
Chapter 1 Introduction 18 Feridex is a dextran-coated ION that successfully obtained the food and drug administration (FDA) approval and made it into the clinic. In order to obtain new features, synthetic polymers emerged to bring distinctive properties than those offered by natural polymers. For example, polyethylene glycol (PEG) coating provides NPs with high water solubility, improved biocompatibility, and enhanced blood circulation time (Figure 4).37,38 Polylactic acid (PLA) coating contributes to enhancing the biocompatibility and biodegradability of the NPs and exhibits low toxicity.38 Polyacrylic acid (PAA) coating is also commonly used because it offers great possibilities for bioconjugation due to the large amount of carboxylic groups available for further functionalization. Figure 4: Examples of polymers use for the coating of IONs. Among macromolecules, liposomes are useful assemblies to encapsulate NPs when the loading of NPs need to be increased, for example, to achieve better contrast in MRI or higher temperatures in magnetic hyperthermia.23 The bilayer structure can encapsulate hydrophobic and hydrophilic substances, such as IONs, drugs, or imaging probes. In general, the structures composed of magnetic NPs encapsulated within liposomes are usually referred to in the literature as magnetoliposomes.39 1.2.3 NP Functionalization: Click Chemistry Apart from enhancing biocompatibility and achieving water dispersions of IONs, coating molecules can offer ˊanchorsˊ available for further functionalization.40 The current challenges of nanomedicine requires nanomaterials with sophisticated structures that bear targeting molecules, multimaging probes, and cargo release with stimulus-driven mechanisms.41 Therefore, it is of fundamental importance to develop chemistry strategies that enable complex surface modifications such as the attachment of biomolecules to NPs.
Chapter 1 Introduction 19 NPs display polydispersity in size, morphology, and coating coverage, resulting in a high variability of physicochemical properties that hampers the homogeneous conjugation across the NP population. Moreover, the reaction between the NPs and the molecules of interest is interfacial in nature and is affected by factors such as density of ligands on the NP surface, loss of colloidal stability during reaction, and charge repulsions, resulting in low yields of conjugates.42 Additionally, characterization of hybrid inorganicorganic conjugates may be difficult,20,42 and therefore it is essential to employ synthetic procedures that are easy to control, reproducible, and with a broad scope. In 2001, Sharpless introduced the new concept of ‘click chemistry’,43 the main philosophy of which relies on focusing the synthetic effort on the functionalities with desired properties rather than achieving complex structures. In order to provide an adequate toolbox of chemical transformations, criteria was established for a reaction to be considered as click:43 “[to] be modular, wide in scope, give very high yields, generate only inoffensive byproducts that can be removed by nonchromatographic methods, and be stereospecific (but not necessarily enantioselective)…include simple reaction conditions (ideally, the process should be insensitive to oxygen and water), readily available starting materials and reagents, the use of no solvent or a solvent that is benign (such as water) or easily removed, and simple product isolation. Purification, if required, must be by nonchromatographic methods, such as crystallization or distillation, and the product must be stable under physiological conditions.” These very stringent criteria are actually fulfilled only by some chemical transformations:43 additions to carboncarbon multiple bonds, such as epoxidation, dihydroxylation, aziridination, sulfenyl halide addition, and Michael addition chemistry, nucleophilic substitution chemistry, such as ring-opening reactions of strained cycles, cycloadditions of unsaturated species (1,3-dipolar cycloadditions) and DielsAlder reactions, and carbonyl chemistry of the “non-aldol” type, such as formation of ureas, thioureas, aromatic heterocycles, oxime ethers, hydrazones, and amides.
Chapter 1 Introduction 20 1.2.4 1,3-Dipolar Cycloaddition Cu(I)-catalyzed azidealkyne cycloaddition (CuAAC)44 is a variation of the thermic reaction known as azidealkyne cycloaddition. Among those considered as click reactions, CuAAC is the most popular and commonly employed and it is sometimes referred solely as the click reaction.42 The Huisgen 1,3-dipolar cycloaddition between azides and alkynes leads to 1,2,3-triazoles in quantitative yields, and if catalyzed by Cu(I), the reaction proceeds ~108-fold faster at room temperature, and forms regioselectively 1,4-disubstituted triazoles (Scheme 1). The triazole ring possesses high stability towards hydrolysis, redox reactions, and temperature, and it can be considered an artificial analog of the amide bond,45 as it forms hydrogen bonds with water molecules similarly to amide linkages. The CuAAC is not affected by changes in temperature, solvents, and pH. Therefore, it has shown great scope in bioconjugation.46 The reaction is neither oxygen- nor water sensitive, since Cu(I) is generated in situ with reductant species such as ascorbic acid. CuAAC has been successfully employed for the functionalization of carbohydrates, peptides, nucleosides, and non-natural molecules, such as dendrimers.47–49 Scheme 1: CuAAC reaction between an alkyne and an azide moiety to give access to 1,4-triazole. Due to its attractive features, the CuAAC has been employed for the functionalization of IONs. For example, Mathur and coworkers50 functionalized the surface of magnetite with biotin and a cysteine protease inhibitor by CuAAC, and showed the promise of these nanohybrids for the caption and detection of proteases. In another study, Brougham and coworkers51 reported for the first time the grafting of a glycopeptide on the surface of IONs by CuAAC. Kjems and coworkers52 developed IONs coated with PEG and a specific targeting peptide using CuAAC and showed promising results of receptor-mediated endocytosis in in vitro experiments.
Chapter 1 Introduction 21 1.2.5 DielsAlder Reaction One of the most interesting click reactions is the DielsAlder cycloaddition because it offers thermal reversibility.43 DielsAlder reaction was first described by Otto Diels and Kurt Alder in 1928,53 for which they were awarded the Nobel Prize in Chemistry in 1950. The reaction is a [4+2] cycloaddition between a conjugated diene and a dienophile to form a substituted six-membered ring. If there is a non-carbon atom present in either the diene or the dienophile, the reaction is called a hetero- DielsAlder reaction.54 The mechanism of the reaction is assumed to proceed via a single cyclic transition state. A variety of dienes can be employed in the DielsAlder reaction (Figure 5), for which the major requirement is a cis conformation within the double bond. Regarding the electron requirements, the normal electron-demand DielsAlder reaction is a reaction between an electron-rich diene, such as ciclopentadiene, and an electrondeficient dienophile, such as maleic anhydride. However, if the diene has electronwithdrawing groups (EWGs) as substituents, and the dienophile bears electrondonating groups (EDGs), an inverse electron-demand Diels–Alder reaction can take place. Figure 5: Examples of good and poor dienophiles and dienes in the Diels Alder reaction. When an unsymmetrical diene and dienophile react, two different regioisomers can be formed depending on the positions of the substituents. Because Diels–Alder reactions are concerted cycloadditions, the stereochemical information of the reactants is retained within the products, i.e. if the dienophile employed has substituents with Z
Chapter 1 Introduction 22 conformation, the adduct product will have the substituents with anti stereochemistry. Moreover, if the dienophile is unsymmetrical, two transition states are possible: the endo and exo transition state, each leading to adducts of different stereochemistry. In the endo transition state, the substituent on the dienophile is oriented towards the diene, whereas in exo it is oriented away from it. For normal electron-demand DielsAlder scenarios, with electron-withdrawing substituents such as carbonyls attached to the dienophile, the endo transition state is typically preferred, despite often being the more sterically hindered one (Scheme 2). This preference is known as the Alder rule, and it is based on the secondary orbital interactions and the overlap of π orbitals.54 Scheme 2: Diels Alder reaction with the formation of exo and endo products. For biomedical applications, the DielsAlder reaction of furan as the diene with maleimide as the dienophile is the most popular (Scheme 3).55 The reason is related to the low temperature that this adduct requires for undergoing the retro-DielsAlder reaction, although this is dependent on the substituents on both moieties.56 This characteristic offers the possibility to obtain temperature-responsive materials.
Chapter 1 Introduction 23 Different molecules containing furan and maleimide moieties have been extensively used in polymer chemistry, as demonstrated in the vast literature on this topic.57–59 Scheme 3: Diels Alder reaction between a furan and a maleimide moiety to give access to a 6-membered ring adduct. The application of the furanmaleimide reactions to IONs is a much more recent strategy. IONs offer the possibility of triggering the retro-DielsAlder reaction taking advantage of the magnetic properties to initiate the increase in temperature. The temperature needed to produce the retrocyclization is dependent on the particular characteristics of the formed adduct, for example, usually endo products require lower temperatures of 30 to 50 °C than the exo isomer to undergo the reaction.55 Moreover, the electronic characteristics and the position of the substituents on the furan and maleimide moieties also affect the adduct stability. Theoretical and experimental studies have shown that furan dienes substituted with EDGs in the second position are the most promising in obtaining reversibility, while EDG substituents on the fourth position in the furan ring usually give access to high energy adducts that cannot undergo the retrocyclization.56 Two different examples are found in the literature that employ furan and maleimide moieties and IONs.60,61 Kirschning and coworkers61 reported on the preparation of IONs with maleimide functional groups. In this work, commercially available magnetite NPs were reacted with maleimide-containing silane ligands, followed by a DielsAlder reaction with furan-modified coumarin molecules as a model system for the quantification of the maleimide functional groups. Moreover, the maleimide-NPs were functionalized with a furan-modified Ansamitocin, a drug with antitumoral activity. The authors studied the release of the drug by conventional heating in an oil bath and by magnetic hyperthermia. The results showed a higher release rate under magnetic hyperthermia than with conventional heating, and the proposed reason
Chapter 1 Introduction 30 population.78 The labeling efficiency can be assessed quantitatively by Fe staining, i.e. Prussian blue (PB) assay, photothermal microscopy, or flow cytometry (if a fluorophore is employed), in order to confirm the cellular dose. Figure 9: Different dose concepts for cell tracking applications: cellular, delivered, and exposure dose. The amount of internalized Fe depend on the particular physicochemical properties of the NPs and on the cell type employed, but they are generally in the range of 330 pg Fe/cell.77 As a reference, Park reported uptake values of 18 pg Fe/cell employing Resovist (FDA approved ION) and PLL.79 However, new formulations of IONs have been recently reported in the literature to achieve a higher cellular dose77 and, consequently, long-term detectability by MRI. IONs coated with pullulan and ethylenediamine reported by Tabata80 showed 65 pg Fe/cell, a very high uptake value also reported by Ni81 and coworkers with IONs coated with PLL. 1.3.4 Limitations of IONs for Cell Tracking Despite IONs offering a great opportunity to label stem cells, they also suffer from certain limitations.75 The first issue is related to the MRI detection: when the cells proliferate the ION cargo divides into the daughter cells, and therefore the detection may be compromised. Moreover, the cell migration in vivo leads to a low density of labeled cells in the area of interest that can be below the detection limit, since detecting a single stem cell is not yet possible. The second limitation concerns the lack of
Chapter 1 Introduction 31 functional information of the cell from the IONs. On one hand, IONs result in no different MRI signal if the stem cell differentiates into other cell types, and thus the use of complementary techniques, such as immunohistochemistry or confocal chemistry, is needed to access that information. In the case of cell death, the situation is equivalent: IONs will give no distinguishable MRI signal from living cells. Furthermore, when the dead cells are cleared off, they are incorporated by macrophages, thus resulting in a risk of misinterpretation of the MRI signal. The need for multimodal probes and techniques is mandatory for cell tracking, as there is complex information that needs to be addressed. Cell tracking is still in the early stages and current efforts are focused on multimodality detection of transplanted stem cells to enhance the reliability of the obtained data.82 1.3.5 Hyperthermia Hyperthermia treatment is based on a temperature increase to cure a medical condition, nowadays mainly investigated for cancer treatment. The belief of heat as a medical tool for therapy dates to many centuries ago to the time of Greeks, Egyptians, and Romans. Parmenides stated in 500 BC:83 Give me a chance to create fever and I will cure any disease. It was in 1898 when F. Westermark conducted the first clinical trial to treat cervical cancer by raising local body temperature by the application of hot water. The Swedish gynecologist noted excellent response in seven patients.84 Since then, many clinical trials on hyperthermia have been conducted for the treatment of different types of cancer, such as glioblastoma multiforme,85 sarcoma, or breast cancer.85 The specific mechanisms behind hyperthermic cell damage are still unknown, though it is believed that the key step is protein denaturation.86,87 Cell death pathways are different depending on the temperature. When the temperature rises to around 4145 °C, cells are involved in the apoptosis pathway. Apoptosis is a type of cell death present in normal tissue homeostasis that does not result in an inflammatory response.88 Investigations are undergoing to accelerate the apoptosis rate in tumors through treatment with heat,3 radiation,89 or chemotherapy.90 On the contrary, when
Chapter 1 Introduction 32 the temperature rises above 46 °C, cells suffer necrosis and the treatment is known as thermal ablation. Necrosis is a premature cell death pathway and therefore result in an inflammatory response.88 Thermal ablation is harmful and presents more side effects when compared to mild hyperthermia treatment, and therefore the latter is preferred. Tumor cells have shown greater sensitivity to heat when compared to healthy cells.83 There are two main aspects that contribute to the higher vulnerability of tumors cells to thermotherapy. First, cancer cells are dividing faster in mitose phase and therefore protein denaturation deeply affects the synthesis and repair of the DNA.87 Second, the tumor architecture is characterized by low vessel density as a consequence of rapid growth, which results in low blood flow with less heat dissipation capability.91 The resistance of tumors to chemo and radio therapies frequently cause failure in the treatment. Hyperthermia has been proven to have a synergic effect with either chemotherapy or radiotherapy,92 being more effective than those therapies alone. The therapeutic effect of the delivery of radiation and/or drugs was found to be enhanced with increasing temperature.86 As a consequence of hyperthermia, the oxygenation of tumors rises and the penetration of radiation is increased. On the other hand, the blood flow is also increased by heat, improving the delivery of drugs into the tumor. Hyperthermia treatment is classified into three types according to the treated area: whole body hyperthermia; regional hyperthermia, for advanced cancer treatment by perfusion or microwaves; and local hyperthermia, mainly used for volumes smaller than organs. The latest is the least invasive technique. 1.3.6 Magnetic Hyperthermia Local hyperthermia uses heat mediators known as antennas that can emit microwaves, ultrasounds, or radio waves.93,94 Magnetic hyperthermia (MH), or magnetic fluid hyperthermia, uses magnetic materials, mainly iron oxide NPs, as antennas to transform electromagnetic energy into heat when placed under an alternating magnetic field (AMF).95 The radiation employed in MH must be set in the range of radio-frequency within a few kHz to one MHz.96 These frequencies guarantee that no
Chapter 1 Introduction 33 harmful effects occur while ensuring sufficient penetration depths to access internal organs and tissues, in contrast to other radiation techniques such as microwave or photothermal. MH is mainly applied to the treatment of solid tumors (Figure 10),95 and this research field has grown exponentially in the last ten years (Figure 11). Figure 10: ION-mediated magnetic hyperthermia for the treatment of solid tumors. Figure 11. Scientific articles published in the last ten years using ˊmagnetic hyperthermiaˊ as search term. Web of Knowledge 15.08.16. The conversion of magnetic into thermal energy in MH can be explained by different mechanisms regarding the magnetic material and experimental conditions employed.3,95 If the magnetic material is multi-domain, such as either ferri- or ferromagnetic NPs, the mechanism is governed by hysteresis losses. If the magnetic material is single-domain, e.g. superparamagnetic IONs, the dissipation of heat is promoted through relaxation losses of different nature: Néel and Brownian relaxation. Both relaxation modes depend on the alignment of the particle’s magnetic moment in
Chapter 1 Introduction 34 the direction of the applied magnetic field, and with the reorientation to the equilibrium once the magnetic field ceases. However, Néel relaxation is related with the reorientation of the magnetic moment while the particle itself remains fixed, while Brownian is caused by the friction of the particle with the embedded medium as consequence of the torque provoked when the magnetic moment aligns with the applied magnetic field. On one hand, Néel relaxation is highly size-dependent, as by decreasing the particle size the energy barrier for the magnetization reversal also decreases. On the other hand, Brownian relaxation is also size-dependent but it is mainly governed by the viscosity of the dispersant solution. Both Néel and Brownian mechanisms contribute simultaneously to the thermal energy production. The heating capability of NPs in MH can be defined by several terms, the most common one is known as specific absorption rate (SAR),97 expressed in W g1: SAR = 𝑐∆𝑇 𝑚Fe ∆𝑡 (1) where c is the heat capacity, and ΔT is the temperature increment in a certain time (Δt), and mFe is the mass of Fe. SAR depends on the intrinsic physicochemical characteristics of the magnetic material, but also on the parameters of the measurement, such as frequency and amplitude of the applied magnetic field or concentration of the magnetic fluid. Comparisons from different materials in the literature can be challenging due to diverse measuring parameters, and there is a need for standardization protocols.95 Alternative expressions for the characterization of heat production have been proposed, such as intrinsic loss power98 or effective specific absorption rate.99 The magnetic performance of the fluid in MH governs the dosage needed in order to achieve a desirable increase in temperature. Recently, significant efforts have been devoted to the synthesis and design of nanomaterials for MH applications.41 The most studied composition is the superparamagnetic iron oxide due to the high biocompatibility, low-cost production, and magnetic response.100 Other formulations have been studied in order to increase the heat generation, for example substituted ferrite NPs with zinc, nickel, cobalt, and manganese.66,100–102 However, safety concerns about exogenous ions are high, and iron-based NPs are often preferred.103
Chapter 1 Introduction 35 The physicochemical properties of nanomaterials that affect the heat production are mainly chemical composition, particle size, and core morphology.104 The particle size determines the magnitude of the magnetic moment and the saturation magnetization of the NPs, and a direct relationship has been found in the literature between the particle size and SAR within the superparamagnetic range.95,105 Hergt and coworkers showed the optimal particle size at the transition between superparamagnetic and ferrimagnetic behavior.106 In IONs, this region corresponds to sizes around 20 nm.105 As an example, MagForceTM is a company working in clinical trials for the treatment of glioblastoma by the administration of dextran-coated IONs with sizes of 15 nm followed by the application of MH. As mentioned, the morphology of NPs also plays an important role, as magnetic anisotropy is a key factor on MH.95 Shape anisotropy can enhance the heat production of NPs composed by the same chemical identities but with different geometries. Recently, Srikanth and coworkers found great differences in heat production of spheres and octopods of iron oxides.107 Pellegrino and coworkers108 also showed an increased heat production for nanocubes composed of iron oxides. The heat production of IONs is usually evaluated as the macroscopic temperature increase. However, several studies have shown that the local temperature surrounding the ION’s surface is higher than that observed on a global scale.109,110 Pellegrino and coworkers110 designed a system based on IONs stabilized with PEG polymer chains of different lengths bound to a fluorophore through a heat-sensitive azo group. The amount release of the fluorophore was found to be dependent on its distance from ION surface, suggesting that the vicinity of IONs experienced the highest temperature increase when located under AMF. Moreover, the authors found that the local heat production decreases exponentially with distance from ION surface. These findings shed light on the use of IONs for drug delivery triggered by MH, as the release of molecules can be tuned with designed NPs.
Chapter 1 Introduction 36 1.3.7 Drug Delivery Nano-sized materials have emerged as promising vehicles for drug delivery applications.111 Nanomaterials have the potential to reduce side effects, by increasing the selectivity to the target tissues, of drug candidates that exhibit good therapeutic efficacy but fail in systemic toxicity. Moreover, nanomaterials can increase the lifetime of drugs in the bloodstream due to the protection they give to the drug against hydrolysis. Requirements for drug delivery systems are known as LADME, standing for liberation, absorption, distribution, metabolism, and excretion (Figure 12). Figure 12: LADME processes that nanocarriers undergo after administration to a host organism. 1.3.8 Magnetic Nanohybrids Magnetic systems that have emerged as carriers for drug delivery applications include single and cluster functionalized IONs, and secondary supramolecular structures such as magnetoliposomes, magnetic polymersomes, and magnetomicelles.2,112 Magnetic nanocomposites have different architectures with embedded NPs either in the core or at the surface of the system depending on the interaction, covalent or non-covalent, between the inorganic NPs and the organic materials.
Chapter 1 Introduction 37 The magnetic response of the NPs opens the possibility of detection by MRI, guidance to the desired location by application of magnetic fields, temperature increase by hyperthermia, and drug release on command triggered by heat production.2,41,66 Therefore, magnetic NPs can act as theranostic probes, providing assistance in both therapy and diagnosis simultaneously.41 The strategy of clustering individual NPs in supramolecular assemblies allows increasing the magnetic response while maintaining the superparamagnetic behavior. However, hydrodynamic sizes below 200 nm are optimal in order to avoid opsonization and subsequent elimination by the reticular endothelial system (RES).113 Synthesis methods of IONs were discussed in the previous Section. The hybridization of inorganic NPs with polymeric materials can be performed one-pot or in a further functionalization step after magnetic core formation. The main synthesis methods of organicinorganic hybrid nanocomposites containing magnetic NPs consist of emulsion, solvothermal, and sol-gel techniques.11 For drug delivery applications, the physicochemical properties of the resulting supramolecular hybrids dictate the pharmacokinetic profile, and special attention must be paid to magnetic loading, biodegradation of organic and inorganic counterparts, polydispersity index, particle size distribution, and surface charge. 1.3.9 Drug Loading The incorporation of the selected drug into the nanohybrids can be accomplished by several approaches including covalent and non-covalent linkages between the drug and the nanocarrier (Table 3). Table 3. Interaction-driven forces for the non-covalent incorporation of drugs into magnetic nanocarriers and stimuli-responsive bonds most used in covalent drug functionalization. Non-covalent Covalent Hydrophobic interactions Thermodegradable bonds Coordination chemistry pH degradable bonds Physically trapped in pores Enzymatically cleavable bonds
Chapter 1 Introduction 38 1.3.9.1. Non-Covalent Conjugation The non-covalent approach for drug loading in nanocarriers relies on low-energy interactions, such as hydrogen bonding, dipole interaction, the hydrophobic effect, and coordination chemistry.2 Nature is the best example of creating sophisticated structures based on supramolecular chemistry. The major advantage of this strategy is that there is no need to chemically modify the drug, which could lead to loss of the therapeutic effect. Consequently, the synthetic effort is considerably low in comparison with covalent modifications. The conjugation between a drug, magnetic NPs, and organic polymers can be very complex, and engineering systems with time-controlled release, i.e. no premature drug release, can be very challenging. For example, Chourpa and coworkers114 showed recently IONs loaded with a complex of iron and doxorubicin (doxo). Fe2+ acted as a bridge between doxo and the NPs. However, the drug-release profile reached 60% after 2 h, and when administered in vivo, the therapeutic performance was equivalent to that of the free drug. The premature release of a drug loaded into nanocarriers implies obtaining the same therapeutic and toxic effects as when administering the free drug. This is one of the major challenges to be overcome for the success of nanosystems in drug delivery. However, some examples in the literature have already shown promising results as magnetic drug delivery systems with the non-covalent approach. An example of a successful nanocarrier with doxo was reported by Yang and coworkers.115 The NPs displayed hydrodynamic diameters in the range of 140180 nm and were prepared by the interaction of negatively charged IONs with positively charged doxo and silk fibroin. The authors stated that the particle formation is driven by electrostatic and/or hydrophobic interactions between the three components, and that there is an optimal doxo/NP ratio. The synthesized nanocarrier showed good internalization in in vitro experiments with drug-resistant cell lines and very high rates of tumor regression in in vivo experiments. Non-commercial IONs coated with dextran were also tested after addition of positively charged doxo.116 The doxo release only reached 10% over the first hours at neutral pH,
Chapter 1 Introduction 39 while at the acidic pH of 6, the released increased to 45%. This is an example of pH-responsive drug release. The NPs were tested in rabbits and showed a better therapeutic performance than free doxo. Recently, nanosystems that trigger the release by MH have been actively studied.117– 119 AMF is much less absorbed by human tissues than other radiations such as light or microwaves. A greater penetration depth is therefore possible with AMF, offering a suitable therapy for in vivo applications.117 The heating by AMF of non-covalently bound systems is believed to enhance the diffusion rate of the encapsulated drugs, resulting in a notable increment in the release of the drug after AMF irradiation. These systems are still at an early stage, and model molecules such as fluorophores are sometimes employed for the sake of simplifying the quantification of the released amount. For example, Parak and coworkers117 recently proposed a system of microcapsules with a mean size of 4.6 µm prepared by layer-by-layer methodology. Magnetic nanocubes were placed in the shell of the structure, while the core was loaded with dextran cascade blue, a fluorophore, as a model molecule. The technology used was based on the assembly of polyelectrolytes with opposite charges, and the authors showed that after irradiation with AMF the outer shell was partially disrupted due to the effect of the magnetic NPs, but the release of the cargo from the microcapsule was only partial. Another example of MH-induced drug delivery was recently reported by Ménager and coworkers.119 In this study, magnetic NPs were used as individual cores with molecularly imprinted polymers, onto which doxo was loaded by hydrogen bonds in the binding sites. After AMF treatment, the NPs showed a doxo released of 60% while control NPs (no AMF irradiation) released at 15%. Moreover, in vitro studies with cancer cells showed a reduction in the viability after AMF that caused the release of doxo. An example with in vivo data was reported by Tseng and coworkers, who prepared nanohybrids with sizes varying from 70 to 160 nm.120 The supramolecular structures were composed of Zn-doped magnetite coated with adamantane-modified
Chapter 1 Introduction 46 is fundamental to consider not only the given inorganic core and organic/inorganic coating, but also the composition and stability of the formed biological corona. The NPs after production are referred to as ˊsynthetic entitiesˊ, while after interaction with biological fluids, and thus formation of a protein corona (PC), NPs are considered as ‘biological entities’ (Figure 15).140 Therefore, it is important to consider the composition of the biological corona in the early design of NPs to obtain the expected properties and performance of the NPs. Figure 15: Synthetic entity of NPs after synthesis and purification (left), and biological entity after the administration of NPs to a living organism (right). It is still not possible to predict the PC of NPs. The complexity of the NPs together with the intrinsic complexity of biological fluids hamper the use of traditional characterization techniques for in situ detection. The development of new methods are crucial, and will be discussed in the following.20,137 The most studied type of biomolecules in interaction with NPs are proteins, and other non-protein coronas such as those formed by lipids of natural organic matter are far less understood.141,142 1.4.1 Protein Corona The magnetic performance of IONs is mainly governed by the inorganic core, with physicochemical parameters such as core size, doping ions, and crystallinity playing the most important roles. However, once the NPs are within a living organism, such properties may be jeopardized due to dissolution, aggregation, or degradation of the NPs. Their performance in the required application, e.g. as contrast agents in MRI or as antennas for MH, may be compromised depending on the NP environment.143 The outer layer composed either of organic or inorganic materials is responsible for the
Chapter 1 Introduction 47 colloidal stability of the NPs and it also offers possibilities for anchoring diverse molecules such as imaging probes, polymers, and receptors. The synthetic coating is in direct contact with the medium and therefore constitutes the first point of contact for the biomolecules to interact. The so-called PC is formed when proteins interact with NPs.141 The definition of PC often refers to two different coronas, depending on the strength of the protein biding to the NP surface. The protein layer bound the closest to the NP, known as hard corona, is the most stable and it is in a long-lived equilibrium state. The hard corona represents a fingerprint of the NP fate.144 The outermost protein shell, known as soft corona or protein cloud, is constituted by proteins loosely bound to the hard corona, which are in a rapid equilibrium exchange with the molecules in the medium.144 Cedervall and colleagues139 introduced the PC to the NP community in 2007, suggesting size exclusion chromatography, surface plasmon resonance, and isothermal titration calorimetry as the characterization techniques to study the binding affinities between NPs and proteins. However, due to the weak interaction between the hard and the soft corona, the characterization and the relevance of the latter remains not fully confirmed, and sometimes both terms are merged in the general concept of PC.141 Stauber141 and coworkers published a review in 2015, where they affirmed: ‘…nanoparticle corona represents a still unresolved hot topic, with high scientific and economic relevance’. The phenomenon of the PC is still not predictable and the majority of the studies were made in simplistic scenarios such as culture medium or blood plasma,145–147 with studies in biological fluids from lung or brain now emerging.147,148 The PC formation is related with the physicochemical properties of the synthetic NP but is also influenced by externals factors such as temperature,149 time of exposure between the NPs and the biomolecules,150 and the concentration of NPs in the physiological media.140 Additionally, intrinsic chemical characteristics of the NPs also play a fundamental role governing protein adhesion: the hydrophobicity of the coating
Chapter 1 Introduction 48 has an impact on the PC, with the general assumption that the more hydrophobic the surface, the less protein interaction occurs.139,151,152 The surface functionalization139 and charge,150 and the size of the NPs153 also have an impact on the final composition of the PC. Although several studies point out the role of the aforementioned factors governing the PC, there is still not enough knowledge to predict the particular protein corona composition for a given NP.141,144,150,154,155 The PC has a high impact on the NPsˊ blood circulation time, cell uptake,144 and also on the cell-targeting efficacy,156,157 thus its prediction would assist in the design of new nanomaterials. There are some examples in the literature of guiding the PC formation in order to target diverse diseases and/or organs.158 For example, Hoshino et al.159 showed that imprinted polymeric nanoparticles were able to capture specific peptides present in the blood stream, and therefore acted in vivo as synthetic nanoparticles with antibody-like affinity and selectivity. Wentworth and coworkers160 modified quantum dots with small molecules, oxysterols, that induced a controlled protein misfolding, resulting in nanomaterials with in vitro targeting properties. 1.4.2 Uptake by Cells After the formation of the biological entity, the biomedical application of the NPs may require internalization within the population of cells of interest in order to accomplish the desired effect. For example, in drug delivery or in cell tracking applications the NPs must be internalized to release the therapeutic molecules and to label the cells, respectively. Together the physicochemical characteristics of the NPs (size, shape, surface charge and hydrophobicity, and surface functionalization)161,162 and specific cell properties (cell type, cycle phase, lipid membrane, etc.) govern the NPcell interactions (Figure 16).163 Engineered NPs have to overcome several barriers in order to be internalized by cells. The cell membrane is the first physical barrier that separates the NPs from the cell, and it hinders the diffusion of complexes larger than 1 kDa.164 There are two different modes for crossing the cell membrane: direct translocation and endocytosis.165 The
Chapter 1 Introduction 49 first involves the direct transfer of extracellular molecules into the cytosol without the formation of vesicles. On the other hand, the endocytosis process is employed by large polar molecules that cannot simply pass through the hydrophobic cell membrane. These processes are subdivided into specific categories: phagocytosis, macropinocytosis, caveolar-mediated endocytosis, clathrin-mediated endocytosis, etc., regarding the different biomolecules involved in the signaling and engulfing of the cell membrane. It is important to consider for engineered NPs that endocytosed materials are trafficked into the cytosol by endosomes and lysosomes, which subject NPs to an acidic pH (4.86.2) and the presence of hydrolytic enzymes.166 Figure 16: Physicochemical characteristics of NPs that affect the internalization processes in cells. The size and shape of the NPs dictate the rate and mode of the endocytosis process. Champion and Mitragotri167 studied the influence of the size and shape of polystyrene NPs on the phagocytosis process. For example, in the case of elliptical disc NPs, if the contact between the cells and the NPs was formed by the short axis, the phagocytosis process was completed in minutes, whereas if the interaction was accomplished by the long axis, the phagocytosis did not occur. These findings shed light on the effect of the geometric anisotropy in nanomaterials in phagocytic processes. Chithrani et al.168 studied spherical and rod-shaped gold nanoparticles of sizes varying from 14 to 100 nm. They found that with spherical NPs the maximum uptake was achieved with 50 nm
Chapter 1 Introduction 50 NPs, and that the rod-shaped NPs were less efficiently internalized by Hela cells than their counterparts with spherical morphology. A maximum internalization rate was also found at 50 nm for other compositions of NPs such as silica169 and single-walled carbon nanotubes.170 Apart from size, the surface charge also plays a role in internalization. In general, cationic NPs are internalized with higher rates in comparison to negatively charged or neutral NPs.165 This is due to favorable electrostatic interactions between the positive charges on the NPs and the negatively charged species on the cell membrane.171 However, depending on the cells and the endocytic mechanism negatively charged NPs can also be successfully internalized.172 NPs can be functionalized with ligands including antibodies, aptamers, peptides, and small molecules in order to target a desired cell population.164 This strategy consists of targeting a membrane-bound protein or a carbohydrate, and it is mainly used for oncology treatment. The accumulation of nanomaterials to a certain location because of ligandreceptor interactions is known as active targeting.4 Apart from the increase in selective toxicity, the study of NPs with functionalized ligands in oncology gives information about the expression and activity of specific molecules in tumors, and therefore brings knowledge of biological processes to help in the prognosis of the disease.173 The tumor cells overexpress biomarkers on their surface known as receptors that have high affinity for some ligands, such as antibodies, aptamers, and small peptides.174 The expression levels of these receptors vary depending on the tumor type but they are also present in healthy tissues. Therefore, the success of this strategy relies on the appropriate selection of the ligand. Taking advantage of the high affinity and selectivity of antibodies, IONs were encapsulated in micelles functionalized with epidermal growth factor receptor (EGFR), which accumulated in glioblastoma as detected by MRI.175 However, antibody functionalization tends to increase the overall particle size, sometimes preventing effective accumulation in the tumor tissue, and its use may be not cost effective.176 On the contrary, small ligands display the advantages of higher stability, low cost, and nonimmunogenicity.176 The most commonly used are folic acid177 and
Chapter 1 Introduction 51 arginineglycineaspartate (RGD) peptide.178 The conjugation of IONs and folic acid was employed to target diverse cancer cell lines, such as human cervical carcinoma (Hela),179 mouse melanoma (B16F0),180 and human epidermoid carcinoma (KB cells).181 Aptamers182 are single strands of either DNA or RNA with analog binding properties to antibodies but with simple structures, and they were used in combination with IONs to target prostate and colon cancer.183,184 The spacing and density of a given ligand on the surface of NPs affect the internalization process,166 and they directly depend on the NP size.165,185 Small NPs possess low surface area and high curvature that restricts the amount of possible attached ligands. Additionally, the binding affinities of these ligands to the receptors are different depending on their density on NP surface. For low density of ligands on the NPs, the binding affinity is close to the values of the free ligands, and therefore the binding capacity can be too low, leading to inefficient uptake.168 On the other hand, large NPs have a higher surface area available to allocate more ligands, and the binding affinities become high due to multivalence, which may limit the membrane wrapping, also leading to low uptake.185 Chan and coworkers185 employed gold NPs to study the size dependency on receptor-mediated endocytosis, and the authors claim 4050 nm NPs as the ideal size range to achieved active targeting. The field of targeting NPs has grown considerably due to the promise of personalized medicine.186 Studies suggest that ligand-functionalized NPs do not accumulate more in malignant tissues, such as tumors, than non-functionalized NPs, but they are more effectively internalized by tumor cells.187 Despite the great potential of targeting, only a few nanomaterials have progressed into clinical trials. This slow progress is the consequence of high production costs and small therapeutic gains in comparison with bare nanomaterials.188 Events such as the formation of the PC in NPs need to be better controlled in order to avoid hiding the ligand from the cell’s receptor. More studies are needed to point out the relations between the PC formation and the characteristics of NPs in order to predict the events at the biointerface of produced NPs with biological systems.
52
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 53 CHAPTER 2 2 Ultrasmall Magnetic Nanoparticles: MRI performance and in vitro stability
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 54 2.1 INTRODUCTION Ultrasmall superparamagnetic iron oxide nanoparticles (USPIOs), with a mean hydrodynamic diameter below 50 nm, possess characteristics such as biocompatibility, long plasma half-life, and interesting magnetic properties, which make them suitable for a wide range of biomedical applications in both therapy and diagnosis.189 MRI is one of the most used techniques in the medical field for the diagnosis of diverse diseases due to its high spatial resolution, rapid acquisition times, and the absence of exposure to ionizing radiation. However, CAs are frequently employed to distinguish between adjacent tissues, for example to enhance the visualization of tumor morphology or coronary angiography. CAs affect the relaxation time of water protons’ nuclei by two different processes: the longitudinal relaxation or T1, where the contrast obtained is bright or positive, and transversal relaxation or T2, with dark or negative contrast. Commonly, CAs are helpful for the reduction of either T1 or T2. Dual T1T2 CAs would help to distinguish interferences, such as hemorrhagic regions, bond calcification, metal deposits, and susceptibility artifacts,190 leading to a more accurate and early diagnosis.191 Additionally, dual behavior of a single CA platform within the same technique simplifies the acquisition due to identical penetration depths and time scale in both imaging modes. Consequently, dual T1T2 systems have attracted attention in the recent years, and complex nanostructures from coupled materials have emerged in order to fulfill both T2 and T1 requirements, for example iron oxide NPs attached to gadolinium compounds.68,69,192,193 Despite the success of these structures in possessing attractive MRI properties, questions remain that need to be addressed before the clinical application of dual CAs can become a reality.194 Some of such concerns are the requirement of facile synthesis procedures to obtain crystalline material on a sufficiently large scale with the desired magnetic properties. Additionally, interactions between the NPs and biomolecules should be addressed to assess the suitability of the nanomaterial for biomedical applications.195,196 The chemical stability and the behavior of NPs in a biological environment are key factors in biodistribution, toxicity, and their eventual efficiency as imaging probes.197
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 55 In this chapter, a straightforward gram-scale synthesis of water-dispersed USPIOs is presented. Moreover, the protein adsorption on the nanoparticle surface and the aggregation of nanoparticles was evaluated with two samples of different sizes in biological media. The MRI properties of these samples will be also discussed. 2.2 SYNTHESIS OF IONS In order to gain access to NPs in sufficient quantity with a procedure that refrains from the use of both organic solvents and phase-transfer procedures, USPIOs were prepared using a one-step hydrothermal method.198 The magnetite structure was chosen to dope with divalent transition metal ions Zn2+ and Mn2+ to maximize the saturation magnetization.14 Additionally, Mn2+ is known to shorten the T1, mainly through magnetic dipoledipole interactions due to its five unpaired electrons, and thus its incorporation has been shown to lead to dual CAs in some cases.199–201 A mixture of FeCl3•6H2O, ZnCl2, and MnCl2•4H2O was kept at 200 °C during 24 h with ammonia as the precipitation agent and water as solvent. PAA was the coating of choice due to its hydrophilic nature and the great affinity of carboxylic acid groups for Fe, giving access to water-dispersed NPs in one pot without the need of phase-transfer procedures. The USPIOs were purified twice by magnetic separation using water as solvent to yield sample NP-bc (before centrifugation). In order to decrease NP size and increase monodispersity, sample NP-bc was subjected to an additional centrifugation step at 4000 rpm for 12 h, and the collected supernatant gave sample NP-ac (after centrifugation). Notably, although the additional separation step reduces the nanoparticle yield, NP-ac was obtained on a gram scale (Figure 17). In order to shed light on the influence of the separation step on the properties of the nanoparticles, the samples before (NP-bc) and after (NP-ac) the centrifugation were studied in parallel. To gain insight into the composition of the NPs, stoichiometry of both samples was estimated by inductively coupled plasma optical emission spectroscopy (ICP-OES) as Zn0.07Mn0.77Fe2.16O4 for NP-bc and Zn0.07Mn0.86Fe2.07O4 for
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 62 the amount of unreacted Cy3-NH2 was quantified by comparing against a calibration curve of the fluorophore in water (Figure 26). The unreacted amount of Cy3-NH2 was subtracted from the amount placed in the reaction mixture, and assumed to be covalently attached to the PAA in NP-ac. The results obtained showed the success of the peptide coupling in 98% yield when 100 eq of Cy3-NH2 per NP were employed (Table 6), showing that the PAA coating can be employed for NP functionalization with e.g. biomolecules for targeting or drug delivery. Figure 25: FT-IR of NP-bc (red) and NP-ac (black) with the characteristic bands of carboxylic acid moieties stemming from the polyacrylic acid coating: 1650 cm 1 for C=O, 1540 and 1400 cm 1 for CO2 1100 cm 1 for CO2H, and 578 cm 1 for Fe O of the magnetic core. Table 6: Various conditions employed for the coupling of Cy3-NH2, and the yield of functionalized NPs after purification Cy3-NH2 eq µg added µg recovered Yield (%) 100 19 0.33 98 300 57 2.82 95 500 90 13.2 85
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 63 Scheme 5: Peptide coupling between carboxylic acid moieties of the PAA coating and Cy3-NH2. Figure 26: Calibration curve with Cy3-NH2. 2.3 USPIO STABILITY 2.3.1 Chemical Stability One of the requirements for nanomaterials to be successfully applied in the biomedical field is the preservation of their chemical integrity over time and under biological conditions.203 Metal leaching from NPs, for example, has been shown to promote toxicity in some cases.203 Thus, chemical stability of metal nanoparticles implies that no metal ions are released into the solution, and this should not only be evaluated when NPs are stored over time, but also in the presence of biomolecules, such as proteins, vitamins, and lipids. The chemical integrity of NP-bc and NP-ac was evaluated by quantifying free Fe and Mn ions released from the samples during storage in water at 4 °C during 10 months. The results showed negligible metal leaching after 10 months of storage, with 0.03 and
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 64 0.02% of Fe ions and 0.14 and 0.09% of Mn ions released into the storage solution for NP-bc and NP-ac, respectively (Figure 27), showing that these NPs are chemically stable for storage periods of at least 10 months. Additionally, in order to quantify the chemical leaching of NP-bc and NP-ac in a biological context, NPs were incubated for 1 h at 37 °C with rat mesenchymal stem cell (rMSC) culture medium, which has a highly protein-rich composition to hinder stem cell differentiation into other types of cells.204 When NPs are incubated in this biological medium, the release of Fe and Mn ions is increased as compared to the sample stored in water at 4 °C. However, the leached quantities remain small, with 0.42% of Fe ions and 0.53% of Mn ions for NP-bc, and 0.73% of Fe ions and 0.56% of Mn ions for NP-ac (Figure 27). Although comparison with literature-reported materials is difficult due to differences in conditions and types of materials, the values obtained for NP-bc and NP-ac are very low: for example, Wang and coworkers205 recently showed 9% Mn ion leaching for hydrogels loaded with iron and manganese oxides after incubation with phosphate buffer saline (PBS) at pH = 7.4 for 4 h, whereas Yeh and coworkers206 reported 1.3% of Mn ion loss for Mn3O4 nanoplates after 48 h in PBS and 37 °C. As the chemical stability of NP-bc and NP-ac is high, toxic effects attributed to metal ions leaching seem to be of less concern. Figure 27: Percentage of Fe and Mn ions released from NP-bc and NP-ac to storage solution after 10 months of storage in water at 4 °C (NP-bc, NP-ac) and after 1 h incubation in rMSC culture medium at 37 °C (NP-bc protein, NP-ac protein).
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 65 2.3.2 USPIOs Protein Adsorption Although iron oxide NPs are expected to be biocompatible because iron ions are intrinsic in the human body, once they are in contact with a complex medium, such as blood, interactions between the NP surface and proteins may occur.207,208 This phenomenon can affect the biodistribution of the NPs, promote particle aggregation, and result in toxicity.147,209 The physicochemical properties of NPs, such as size and surface charge, have a large impact on protein adsorption.210–213 Therefore, the characterization of NPs in contact with biological medium is of fundamental importance to verify their suitability for biomedical applications. In order to characterize the physicochemical behavior of NP-bc and NP-ac under biological conditions, both samples were incubated with rMSC culture medium. NP-bc and NP-ac were incubated at 200 µg/mL of Fe in the medium for 1 h at 37 °C. The samples were then recovered by centrifugation at 30000 rpm for 30 min, and the pellet was redispersed in phosphate buffer at pH = 7.4. Then, -potential and Dh of the samples were measured by dynamic light scattering (DLS) and compared to the data obtained prior to incubation. There were no significant changes in the -potential of neither sample after incubation (Figure 28A). However, the Dh of NP-bc had increased from 35 to 50 nm, presumably due to adsorption of proteins onto the NP surface (Figure 28B). In contrast, the Dh of NP-ac remains unchanged after the incubation period, indicating that no aggregation between NP-ac and the proteins of the medium took place. In order to quantify the protein adsorption, a bicinchoninic acid (BCA) assay was performed in rMSC culture medium (Figure 29). BCA assay quantifies the total amount of protein in a given sample by absorbance due to the formation of a purple complex of Cu+. The results of BCA assay showed that the quantity of proteins adsorbed onto NP-bc was five times larger compared to NP-ac. This can be attributed to the different physicochemical properties of NP-bc and NP-ac, most likely the hydrodynamic radius and the coating coverage. NP-bc with a large hydrodynamic radius (35 nm) has lower curvature on the surface as compared to the smaller NP-ac, which may facilitate the binding of the mainly bulky proteins of the medium.214 Additionally, the higher amount
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 66 of polymeric coating around NP-ac (39%) compared to NP-bc (20%) could shield the smaller NP from interactions with biomolecules Figure 28: A) -potential of NP-bc and NP-ac before and after incubation with rMSC culture medium at 37 °C for 1 h; B) Dh of NP-bc and NP-ac at 200 µg/mL before and after incubation with rMSC culture medium at 37 °C for 1 h. . Figure 29: Micrograms of proteins adsorbed onto NP-bc and NP-ac (left) after 1 h incubation in rMSC culture medium. Calibration curve (right) with bovine serum albumin (BSA) protein for the BCA quantification assay. 2.3.3 In vitro Studies When NPs come into contact with a more complex medium, such as blood, protein adsorption is known to lead to NP aggregation.215 In order to study the behavior of NP-bc and NP-ac samples in contact with cells, in vitro studies were carried out using rMSCs (Figure 30, left). Sample NP-bc formed large aggregates already after 1 h of incubation (Figure 30, middle), whereas NP-ac remained stable even after 16 h
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 67 (Figure 30, right), rendering NP-ac suitable candidates for cell detection by MRI.216 Clearly, the additional centrifugation step affords NPs that are much more stable in biological medium, showing promise for the use of NP-ac for biomedical applications. In order to test the biocompatibility of NP-ac, lactate dehydrogenase (LDH) and cell count assays were carried out with rMSCs. LDH assay measures the release of the cytosolic enzyme lactate dehydrogenase, which is an indicator of plasma membrane damage. Cell count assay quantifies are used to verify the normal growth of rMSCs. Briefly, rMSCs were exposed to a concentration of NP-ac as high as 200 µg of Fe/mL for a long incubation time of 24 h, subjecting the rMSCs to demanding conditions (Figure 31). Both cell count and LDH viability assays showed no differences between the control rMSCs and those exposed to NP-ac, highlighting the good biocompatibility of the sample. Figure 30: Optical microscopy images of rMSCs (left), after incubation with NP-bc for 1 h (middle), and with NP-ac for 16 h (right). Figure 31: A) Cell count of rMSCs after incubation with NP-ac for 24 h at 200 µg/mL of Fe. B) LDH viability assay of rMSCs after incubation with NP-ac for 24 h at 200 µg/mL of Fe.
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 68 2.4 MRI MEASUREMENTS The ratio between the longitudinal and transversal relaxation is an important parameter defining CA performance: a high r1 value and a r2/r1 ratio near 1 results in bright contrast in T1-weighted imaging mode. On the other hand, when r2 is the predominant value with a high r2/r1 ratio, the dark contrast is enhanced in a T2-weighted imaging mode. If an intermediate r2/r1 ratio is reached, a dual T1T2 reduction can be accomplished.217 In order to evaluate the efficiency of the nanoparticles as CAs for MRI applications, both transversal and longitudinal r of samples NP-bc and NP-ac were measured at a magnetic field of 1.4 T and 37 °C, giving r2 values of 178 mM1s1 for NP-bc (Figure 32A), and 58.8 mM1s1 for NP-ac (Figure 32B), both higher than that of Feridex and similar to Resovist, with r2 of 41 mM1s1 and 61 mM1s1, respectively, both superparamagnetic iron oxide NPs approved by FDA as negative CAs (Table 7).65 The r1 values of NP-bc and NP-ac are very similar, 13.1 mM1s1 and 13.4 mM1s1, respectively, resulting in very different r2/r1 ratios: 14 for NP-bc and 4.4 for NP-ac, the latter an intermediate value indicating possible dual behavior. Figure 32: A) r1 and r2 of NP-bc at 1.4 T and 37 °C; B) r1 and r2 of NP-ac at 1.4 T and 37 °C.
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 69 Table 7: Comparison of r between Feridex, Supravist, Resovist, Dotarem, and NP-ac. NP-ac was measured at 1.4 T and 37 °C. aMeasured at 1.5 T and 37 °C. bCA in clinical trials. The r of the samples after 10 months of storage in water at 4 °C was re-evaluated, as it is crucial for drug formulations that the properties remain unchanged during storing. The r of stored NP-bc measured at 1.4 T and 37 °C displayed a reduction in both r1, from 13.1 to 8.17 mM1s1, and r2, from 178 to 118 mM1s1, showing that the properties of this sample were significantly deteriorated during storage. On the contrary, NP-ac showed good reproducibility in both r1, displaying values of 13.4 when fresh and 12.0 mM1s1 after storage, and r2, merely changing from 58.8 to 61.8 mM1s1. The r1,2 of NP-ac were not only promising for a dual CA in MRI, but also featured good reproducibility over time, and therefore NP-ac was the sample of choice for further studies on relaxivity (Table 8). Relaxivity measurements of NP-ac were performed at different magnetic fields in order to probe its efficiency as a CA, in both water and 1.6% agar, the latter to mimic tissue density. The r1 obtained for NP-ac is reduced when increasing the magnetic field from 1.4 to 9.4 T, as expected due to the slower electronic relaxation relative to rotational motion at high fields.218 The values are above 10 mM1s1 at clinical fields (3 T or lower) in both water and agar, which are great values to efficiently shorten the T1. Moreover, the r2/r1 ratios are between 4 and 5.5, intermediate ratios that suggest good performance of NP-ac as dual CA in clinical fields. However, at the ultra-high magnetic field of 9.4 T (Figure 33), r1 was significantly reduced to 0.49 mM1s1, limiting the use of NP-ac in T1 mode. Dh (nm) Coating agent r (mM1s1) r2/r1 Contrast Feridex, Endorem 120 Carboxydextran ar1= 4.7 ar2= 41 8.7 Negative bSupravist, SHU-555C 20 Carboxydextran ar1= 13.2 ar2= 44 3.3 Positive Resovist, SHU-555A 60 Carboxydextran ar1= 8.7 ar2= 61 7.0 Negative Dotarem - - ar1= 2.9 ar2= 3.2 1.1 Positive NP-ac 18 Polyacrylic acid r1= 13.4 r2= 58.8 4.4 Dual
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 70 The r1 values are slightly higher in agar when compared to water at the same field, because the rate of spin exchange may increase with slowing molecular motion.219 The r2 is also higher in agar when compared to the results in water in the same field, again due to limited molecular motion, but also because solid environments promote local static field disturbances that shorten the T2. Table 8: r1,2 of NP-ac at 1.4 and 3 T in water and 1.6% agar gel, and at 9.4 T in agar. aSample measured after 10 months of storage in aq solution at 4 °C. Figure 33: T1 and T2 weighted map in 1.6% agar of NP-ac at 9.4 T (left). r1,2 of NP-ac in 1.6% of agar at 9.4 T (right). Phantom images were taken to verify the shown contrast of NP-bc and NP-ac in MRI. The images acquired at a magnetic field of 3 T showed NP-bc serving as a negative CA (Figure 34A). Similarly, when applying a T2-weighted sequence, NP-ac produced a reduction in signal, resulting in dark contrast (Figure 34B). On the other hand, when applying a T1-weighted sequence, the contrast given by the two samples was very different: while NP-bc did not show much difference when compared to water, NP-ac produced a notable increase in signal resulting in bright contrast (Figure 34B), revealing NP-ac as T1‒T2 contrast agent. This dual enhancement along with high stability in biological medium are desirable features for advanced CAs, and they were 1.4 T 3 T 9.4 T Water Agar Water Agar Agar r1 (mM1s1) 13.4 a14.2 a10.2 a12.5 0.49 r 2 (mM1s1) 58.8 a81.6 a50.2 a68.5 43 r 2/ r 1 4.4 5.7 4.9 5.5 87
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 71 only displayed by NP-ac after the centrifugation step. Therefore, sample NP-ac is suitable for dual T1T2 image acquisition at clinical fields, 3 T or lower, but also as a negative CA at a higher field. Figure 34: A) MRI image at 3 T of a NP-bc phantom; B) MRI image at 3 T of a NP-ac phantom. White dashed circles are used in T2-weighted sequences for clarity. In order to evaluate the efficiency of NP-ac as a dual CA, its properties were compared with those of ferrites proposed as dual CAs in the literature, since there is currently no dual CAs commercially available for use in the clinic (Table 9). Although direct comparison is difficult due to differences in the conditions of the measurements, such as magnetic field and the medium, reported dual CAs have similar r2/r1 ratios between 4.4 and 5.4. A comparison of the r1,2 values and the r2/r1 ratios shows that NP-ac displays similar performance as the previously reported dual CAs. However, the advantage of NP-ac is that the synthesis method offers an organic solvent-free alternative to obtaining a dual MRI CA in gram-scale quantity. Table 9: Comparison of r between Feridex, Supravist, Resovist, Dotarem, and NP-ac. NP-ac was measured at 1.4 T and 37 °C. aMeasured at 1.5 T and 37 °C.32 bCA in clinical trials. Ref. Field Coating Synthesis method r1 r2 r2/r1 199 1.5 Polyethylene glycol Seed-mediated growth 13.3 65 4.9 200 0.5 Sodium tartrate Thermal decomposition 27.2 146 5.4 201 4.7 Poly(methacrylic acid) Coprecipitation 6.6 35.9 5.4 NP-ac 1.5 Poly(acrylic) acid Hydrothermal 13.5 58.8 4.4
Chapter 2 In Vitro Stability and T1 T2 MRI Properties 78 with a slice thickness of 1 mm and 1 mm slice gap. An inversion recovery sequence was used for T1, with TR = 24000 ms and TI = 150, 450, 800, 1200, 2400, 4800, 9600, 16000, and 23500 ms. Then, r1 was calculated from the slope of the curve obtained by fitting the T11 values versus the total Fe concentration in mM. For r2 in water, a T2 map was acquired with a multi-echo-multi-sliced (MEMS) sequence of 50 ms echo time, repetition time of 4800 ms and 10 echoes. For r2 in agar, a T2 map was acquired with MEMS sequence of 15 ms echo time, repetition time of 3100 ms and 10 echoes. Post-processing was performed using ImageJ software (Rasband, W. NIH) for the construction of T2 maps, and r2 was calculated from the slope of the curve obtained by fitting the T21 values versus the total Fe concentration in mM. MR imaging: was performed in a 3 T horizontal bore MR Solutions Benchtop (Guildford, UK) equipped with 48 G cm1 actively-shielded gradients. For imaging the sample, a 56 mm diameter quadrature bird-cage coil was used in transmit/receive mode. For the phantom measurements, the samples at different concentrations (between 25 and 500 M in Fe) were dissolved in 200 L of Milli-Q water in 300 L tubes. All MR images of the phantoms were acquired with an image matrix 256 x 252, FOV 60 x 60 mm, 3 slices with a slice thickness of 1 mm and 1 mm slice gap. For T2-weighted imaging a fast spin echo (FSE) sequence with the following parameters was used: TE = 68 ms, TR = 4800 ms, NA = 50. For T1-weighted imaging a FSE sequence with TE = 11 ms, TR = 400 ms, and NA = 50 was used. MRI studies at high magnetic field were conducted on a 9.4 T MR system (Bruker Biospin, Ettlingen, Germany) with 440 mT/m gradients. A quadrature radio-frequency transmit-receive resonator was used for data acquisition. T2-weighted images were acquired using a multi slice multi echo sequence of 7.32 ms echo time, 5.389 s repetition time, 16 echoes, 14 slices, 1 average, FOV of 7.5 cm x 7.5 cm and matrix size of 100 x 100. T1-weighted images were acquired using a RARE-VTR sequence of 8.81 ms echo time, 17.62 ms echo spacing, rare factor 4, repetition times of 900 s, 1500 s, 3000 s, 4500 s, 7000 s, 8500 s, 14 slices, 1 average, FOV of 7.5 cm x 7.5 cm and a matrix size of 200 x 200. Postprocessing was performed using ImageJ software (Rasband, W. NIH).
Chapter 3 Stem Cell Labeling 79 CHAPTER 3 3 Magnetite Nanoparticles for Stem Cell Labeling
Chapter 3 Stem Cell Labeling 80 3.1 INTRODUCTION Stem cells show promise for the treatment of various diseases, such as glioma, ischemic brain injury, Alzheimer´s and Parkinson´s diseases,220 and cardiovascular disease,71–73 as demonstrated by their involvement in more than 360 clinical trials.74 Cell therapy is based on the administration of stem cells, relying on their ability to self-renew and differentiate into most cell types of the adult body. Therefore, the understanding of the needed dose, administration route, and biodistribution of these transplanted stem cells is of fundamental importance in order to develop safe therapies. Non-invasive cell tracking and specific imaging of labeled stem cells in vivo is an ideal methodology to follow the migration and grafting of transplanted cells and to evaluate their fate and therapeutic effect.75 IONs together with MRI constitute a common approach for cell tracking due to the biocompatibility and effectiveness of IONs, and the high spatial resolution, penetration depth, and the lack of ionizing radiations provided by MRI.76 As explained in the Introduction, IONs shorten the transverse relaxation time or T2 in MRI, and therefore create dark contrast in T2-weighted MR images. Clinically approved IONs, such as Feridex or Ferumoxytol, provide low labeling efficiency.221 Although in their natural niches mesenchymal stem cells (MSCs) are phagocytic in nature, during ex vivo cell culture and expansion they lose their phagocytic ability, rendering their efficient labeling a challenge.71,222 A low labeling efficiency limits the use of IONs as magnetic labels to short-term detection, usually referred to as 072 h after cell transplantation.223 Thus, significant efforts have been devoted to developing new ION formulations with different organic coatings to enhance cellular uptake and enable mid- to long-term tracking.77,81,224,225 IONs can be classified as superparamagnetic iron oxide nanoparticles (SPIOs), if the hydrodynamic diameter (Dh) is above 50 nm, or as ultrasmall iron oxide nanoparticles (USPIOs), if it is below. USPIOs have often been studied as CAs because of their enhanced blood half-life when compared to SPIOs, but low cell uptake has hampered their use for cell tracking applications.226,227 The smaller size of USPIOs as compared to SPIOs could result in advantageous properties for cell tracking, such as higher stability in biological
Chapter 3 Stem Cell Labeling 81 fluids, reproducible cell labeling procedures, and homogeneous labeling of the entire cell population.228 In this chapter, the cell labeling performance of SPIOs and USPIOs was studied with MSCs for cell tracking applications. The IONs were studied in regard to their internalization by MSCs and to the contrast achieved in MRI images. 3.2 SYNTHESIS OF IONS In order to apply IONs as magnetic labeling agents in cell tracking, they were synthesized by a hydrothermal method198 using PAA as coating because of the high yield and magnetic response of the NPs, high stability in aqueous medium, and the possibilities the coating offers for further functionalization. Two sets of IONs were synthesized following the same synthetic procedure by hydrothermal method,198 but differing in the purification protocols (Scheme 6).229 The synthesized IONs were purified twice by magnetic separation using water as solvent to render sample SPIOPAA, classified as superparamagnetic iron oxide nanoparticles. The collected supernatant of an extra centrifugation step with SPIO-PAA gave sample USPIO-PAA, classified as ultrasmall iron oxide nanoparticles. Scheme 6: Synthesis route used to produce the two different IONs: after hydrothermal synthesis, SPIO-PAA was obtained. Its purification by centrifugation gave access to USPIO-PAA. SPIO-PAA sample was fully characterized in a previous work by Kolen’ko and coworkers,198 and the data used in this work to compare with USPIO-PAA. The inorganic core composition was confirmed to be magnetite, Fe3O4, by XRD. The diffractogram showed one single phase corresponding to an inverse spinel structure for USPIO-PAA (Figure 35, left). The nature of PAA in the organic coating of SPIO-PAA was confirmed by X-ray photoelectron spectroscopy (XPS). On the other hand, the
Chapter 3 Stem Cell Labeling 82 presence of PAA on USPIO-PAA was confirmed by IR spectroscopy, as identified by the vibrational bands at 1633 cm1 attributed to –CO2H, 1551 cm1 for –CO2, and 558 cm1 for FeO (Figure 35, right). Figure 35: Left: XRD pattern of USPIO-PAA, position and relative intensity (bottom) of the XRD reflections of a Fe3O4 single phase with inverse spinel structure from the COD, pattern code 96-900- 2318. Right: IR of USPIO-PAA with the characteristic bands of carboxylic acid moieties stemming from the PAA coating of 1633 cm 1 attributed to –CO2H and1551 cm 1 for –CO2 , and 558 cm 1 for Fe O. The difference between SPIO-PAA and USPIO-PAA is related with the NP size and the content of organic matter. On one hand, core size measured from TEM images showed values around double for SPIO-PAA compared to USPIO-PAA, 18 and 8.5 nm, respectively (Table 10, see also Figure 36). Figure 36: TEM images of USPIO-PAA.
Chapter 3 Stem Cell Labeling 83 Table 10: Core size from TEM images, Dh, percentage of organic coating calculated from TGA, and Ms, and Hc obtained by VSM for SPIO-PAA and USPIO-PAA. aData for SPIO-PAA are from ref 198. The same trend was observed with the hydrodynamic diameter (Dh) measured by DLS, where SPIO-PAA presented a size of 95 nm, nearly four times that of USPIO-PAA, 24 nm, the latter corresponding to an ultrasmall NP size (Table 10).230 PAA content, calculated by TGA, was found to be 9.3 and 23 wt% for SPIO-PAA and USPIO-PAA, respectively (Table 10, Figure 37 left). As discussed in Chapter 2,229 Dh and the amount of organic coating of IONs play an important role in the colloidal stability of the NPs and their interactions with biomolecules, both important features governing cell uptake. Regarding the magnetic properties, USPIO-PAA featured Ms of 65 emu g1 and Hc of 0.12 Oe by VSM measurements (Figure 37, right). As expected, these values are significantly below those of SPIO-PAA that featured Ms of 81 emu g1 and Hc of 20 Oe,198 as a result of the larger core size. Figure 37: Left: TGA revealing the percentage of organic content in wt% of USPIO-PAA. Right: Hysteresis loop of USPIO-PAA with an inset of the low magnetic field area. Core size (nm) Dh (nm) Coating (wt%) Ms (emu g 1) Hc (Oe) aSPIO-PAA 18 95 9.3 81 20 USPIO-PAA 8.5 24 23 65 0.12
Chapter 3 Stem Cell Labeling 84 MRI performance of USPIO-PAA was then evaluated. Transverse r, r2, of USPIO-PAA was found to be 127 mM1s1 and longitudinal r, r1, 17.7 mM1 s1 at 1.4 T and 37 °C (Figure 38), indicating USPIO-PAA as a three times more efficient CA than the clinically approved SPIO Feridex, which has an r2 of 41 mM1 s1 under the same conditions.65 On the other hand, SPIO-PAA featured values of 202 and 19.3 mM1 s1 for r2 and r1, respectively. The higher r in comparison with USPIO-PAA is in agreement with the larger Ms as a consequence of the larger core size. However, the performance of IONs in cell labeling depends much more on their uptake than on their magnetic properties, since the latter are affected/modified by the cell internalization.143 Figure 38: r1 and r2 of SPIO-PAA (left) and USPIO-PAA (right) at 1.4 T and 37 °C. 3.3 COATING MODIFICATION In general, USPIOs have been reported to be internalized through fluid-phase endocytosis, which results in poor cell uptake.231 As an example, negligible amounts of commercial Ferumoxytol are internalized by MSCs in vitro even when incubated in the presence of protamine. To increase MSCs’ Ferumoxytol loading, the CA has to be used in combination with protamine and heparine, known as the heparin-protamine- Ferumoxytol (HPF) nanocomplex methodology,232 and even then, MSCs only show an iron content of 2.12 ± 0.11 pg Fe/cell. Consequently, in an attempt to achieve receptor-mediated endocytosis, USPIO-PAA was functionalized with targeting molecules. D-Glucosamine (GlcN) was selected for the modification because glucose is
Chapter 3 Stem Cell Labeling 85 known to be biocompatible and has been shown to enhance cellular uptake in other systems (Scheme 7).233,234 Scheme 7: Functionalization through peptide coupling of USPIO-PAA with GlcN molecules in water to yield USPIO-PAA-GlcN. In order to calculate the carboxylic acid moieties available for GlcN functionalization, USPIO-PAA was reacted with the dye Cy3-NH2, following the same procedure as described in Chapter 2.229 Three different quantities of Cy3-NH2 were tested corresponding to 100, 300, and 500 eq to 1 mmol of NPs. By comparing against a calibration curve of Cy3-NH2 in water, the amount of free fluorophore (Cy3-NH2 recovered after purification) was quantified, and found to be 0.33, 2.8 and 13 µg, respectively for 100, 300 and 500 eq (Table 11). The remaining quantity of Cy3-NH2 was assumed to be covalently attached to the PAA coating of the NP. These results suggest that USPIO-PAA has 100 eq of carboxylic acids per mmol of NP available for the reaction by peptide coupling with a 98% yield. Table 11: Carboxylic acid quantification of USPIO-PAA by reaction with Cy3-NH2, Amounts of different equivalents of fluorophore added with the corresponding recovered amounts for each condition. The reaction yield was calculated with respect to added amounts of Cy3-NH2. Equivalents Amount added [µG] Amount recovered [µG] Yield [%] 100 19 0.33 98 300 57 2.8 95 500 90 13 85 After evaluation of carboxylic acids available in USPIO-PAA, GlcN was employed for the reaction with an excess of 1000 eq for the functionalization of USPIO-PAA, following the same synthetic procedure as for Cy3-NH2. The quantification of GlcN in USPIO-PAA-GlcN was performed with the o-phthaldialdehyde (OPA) method (Scheme 8) by comparing the results against a calibration curve (Figure 39).235 The
Chapter 3 Stem Cell Labeling 86 coupling reaction showed high reproducibility in terms of the amount of glucosamine attached to the NP between different batches, with an average of 143 µg GlcN/mg NP (Table 12). Scheme 8: Reaction between unbound GlcN and o-phthaldialdehyde in water at rt that yields to a fluorescent product. Figure 39: Calibration curve between GlcN and o-phthaldialdehyde in water. Table 12: Amount of GlcN attached to USPIO-PAA in three different reactions. µG GlcN/mg NP Batch 1 139 ±17 Batch 2 146 ± 24 Batch 3 145 ± 11 DLS measurements were performed with USPIO-PAA-GlcN to evaluate the surface charge of the NPs. At basic pH, the -potential was 114 ± 14 mV, which after glucosamine modification shifted to 86 ± 7 mV (Figure 40). While USPIO-PAA-GlcN reaches its isoelectric point at around pH 6.0 (0.4 ± 0.1 mV), USPIO-PAA still presents
Chapter 3 Stem Cell Labeling 87 a highly negative -potential at that pH (22.2 ± 0.8 mV), the neutralization confirming that a significant part of the carboxylic acid moieties has reacted with GlcN molecules. Figure 40: -Potential of USPIO-PAA (left) and USPIO-PAA-GlcN (right) at pH = 9. TEM images were acquired after glucosamine modification to ensure that no morphological changes took place after the functionalization procedure (Figure 41), and the core size did not show noticeable changes after the modification. Dh as measured by DLS showed an increase from the original 24 nm to 40 nm after GlcN coupling, with no signs of NP aggregation. Due to the small amount of GlcN molecules attached per NP, the organic content by TGA did not show any significant changes between USPIO-PAA-GlcN and USPIO-PAA, as expected. Figure 41: TEM images of USPIO-PAA-GlcN. 3.4 FE CONTENT IN MSCS In order to foresee the in vivo detection window by MRI, in vitro experiments were performed over time to follow the decrease of internalized Fe as MSCs proliferate
Chapter 3 Stem Cell Labeling 94 3.7 CONCLUSIONS SPIOs (SPIO-PAA) and USPIOs (USPIO-PAA) coated with polyacrylic acid, as well as USPIOs functionalized with glucosamine (USPIO-PAA-GlcN), were studied as labeling agents for MSCs. Dramatic differences were found in the cell-labeling performance of these magnetic NPs. SPIO-PAA showed signs of aggregation in cell culture medium and as a result the uptake was localized and non-homogeneous within the cell population. On the other hand, USPIO-PAA showed good stability in vitro but no significant internalization was observed by MSCs. In combination with polylysine, USPIO-PAA-GlcN displayed great biocompatibility, high cellular dose of 56.5 pg Fe/cell, and sensitive detection in both in vitro and in vivo experiments by MRI, showing promise as labeling agent for cell tracking applications in animal models of cerebral ischemia.
Chapter 3 Stem Cell Labeling 95 3.8 EXPERIMENTAL 3.8.1 Materials and Methods FeCl3•6H2O, NH4OH, polyacrylic acid sodium salt (MW 5100 Da), D-glucosamine hydrochloride, poly-L-lysine (PLL, 1.5 3.0 ×105 molecular weight), potassium ferrocyanide trihydrate (KFe(CN)6•3H2O), 1-ethyl-3-(3- dimethylaminopropyl)carbodiimide, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), OPA, and LDH kit were purchased from Sigma-Aldrich and used without further purification. Potassium bromide (99% for spectroscopy, IR grade) was purchased from Acros Organics. Cy3-NH2 was purchased from Lumiprobe. Trypan blue staining was purchased from STEMCELL Technologies. Ultrapure water was produced by Milli-Q Advantage A10 system (Millipore) and used always when not mentioned otherwise. MSCs were purchased from Cultrex, Trevigen, (Gaithersburg, MD, USA), and were cultured in IMDM (78%), fetal bovine serum (10%), horse serum (10%), penicillin-streptomycin (1%) (Gibco, Invitrogen, Paisley, UK), and amphotericin B (1%) (Sigma-Aldrich, St. Louis, MO, USA). EDTA-trypsin and phosphate buffer saline without Mg2+ and Ca2+ was purchase from Gibco (Invitrogen, Paisley, UK). XRD was performed with a PanAnalytical X Pert PRO MRD system working at 45 kV/40 mA and using a Cu X-ray radiation with wavelengths K1 = 1.5405980 Å, K2 = 1.5444260 Å and K1/K2 intensity ratio = 0.5. In the incident beam path geometry, a Soller slit of 0.04 rad and a divergence and an anti-scatter slit of 1/2 and 1, respectively, were used. On the other hand, a Soller slit of 0.04 rad and Ni large betafilter were used in the diffracted beam path. The detector used was a Pixcell 3D area detector with 255 channels and an active length of 2.511. Measurements were performed in a zero-background signal sample holder in the range 2570 (2 ), with a step size of 0.0098 and time per step of 1500 s in scanning line detector mode. TEM studies were performed using a Titan ChemiSTEM electron microscope and a JEOL JEM-2100 electron microscope, both operated at 200 kV. The samples were prepared by dropping 10 µL of a diluted dispersion of the nanoparticles onto a lacey
Chapter 3 Stem Cell Labeling 96 carbon-coated Cu grid (400 mesh) followed by evaporation of the solvent under vacuum at room temperature. Image processing was performed using Digital Micrograph software (Gatan) and the size distribution of the particles was calculated using ImageJ software. TGA was performed in a TGA/DSC 1 STARe system, Mettler-Toledo, fitted with OmniStar GSD320 gas analysis system (Pfeiffer Vacuum), with 10 K/min gradient from 30 to 900 °C under 30 mL/min of Ar flow. FT-IR spectra were acquired on a Bruker VERTEX 80v FT-IR spectrometer in absorbance mode. A spatula tip of the sample was mixed with 200 mg of KBr and the powder was pressed at 10 tons for 2 min to obtain a transparent pellet. Spectra were recorded at 1.66 hPa with 32 scans and 4 cm1 resolution with deuterated triglycine sulfate detector. The empty holder at 1.66 hPa was used as background and baseline correction was applied to the spectra. Hysteresis loops were measured with a VSM (EV9, Lot-Oriel) in the applied magnetic field range from ‒14 kOe to +14 kOe at RT. Relaxivity measurements: were performed in a minispec mq60 contrast agent analyzer from Bruker at 37 °C and under 1.4 T magnetic field, with standard inversion recovery sequence for T1 and CPMG for T2 calculations. The r1 and r2 were calculated as the slope of the curve obtained by fitting the T11 or T21 values versus the Fe concentration in mM. OPA reaction was measured with BioTek, Synergy H1 hybrid reader at 562 nm. A standard calibration curve was done with BSA standard solution in phosphate buffer (0 to 200 mg/mL). Optical microscopy images were taken with Olympus IX51. LDH assays were performed by measuring the absorbance with Synergy2 Biotek Instruments, Vermont, USA. MRI studies were conducted using a 9.4 T MR system (Bruker BioSpin, Billerica, MA, USA) with 440 mT/m gradients and a combination of a linear birdcage resonator (7 cm in diameter) for signal transmission and a 2 × 2 surface coil array for signal detection.
Chapter 3 Stem Cell Labeling 97 A quadrature volume coil (7 cm in diameter) was also used in phantom studies. MRI post-processing was performed using ImageJ software (W. Rasband, NIH, USA). DLS measurements were performed with SZ-100 nanoparticle analyzer (Horiba). The results of -potential are shown as the average of seven consecutive measurements. The results of Dh are represented in the histograms as intensity scattered light of three consecutive measurements. 3.8.2 IONs Synthesis Procedure SPIO-PAA was synthesized using our previously reported hydrothermal methodology.198 USPIO-PAA was synthesized following a slightly modified procedure. Briefly, 8 mmol of FeCl2•6H2O and 14 mmol of FeCl3•6H2O were dissolved in 10 mL of ultrapure water in a 40 mL PTFE vessel. Next, 15 mL of aq 2530% NH4OH and 0.4 mmol of poly(acrylic acid) sodium salt in 5 mL of water were added to the reaction mixture. The PTFE vessel was placed in a stainless steel autoclave and kept at 200 °C for 24 h under autogenous pressure. NPs were isolated by magnetic separation and redispersed in water by sonication (two times). The resultant NPs were centrifuged at 3000 rpm for 10 min, the supernatant was subjected to an additional centrifugation at 4000 rpm for 12 h, and the supernatant was kept to yield sample USPIO-PAA (1.5 g). 3.8.3 Glucosamine Modification The quantification of free carboxylic acids in PAA coating of USPIO-PAA was performed with Cy3-NH2. For the coupling with GlcN, USPIO-PAA was dispersed in water at a NP concentration of 18.6 mg mL1, and GlcN (2.8 mg, 1000 eq per nanoparticle) was added. Subsequently, DBU (2.5 µL) was added to ensure a basic pH during the reaction, and last, 100 µL of freshly prepared aq. EDC solution (5 mg mL1) were added. The reaction was stirred overnight at room temperature, and then purification was carried out by centrifugation at 7500 rpm during 10 min with Amicon Ultra-0.5 Centrifugal Filter Devices to obtain USPIO-PAA-GlcN (11 mg mL1, 500 µL). Three washing cycles were performed with water, one with aq. 0.1 M NaOH solution, and three more with water, to recover functionalized NPs. The supernatants of all
Chapter 3 Stem Cell Labeling 98 centrifugal purifications were combined and analyzed by the OPA method235 to determine the quantity of unreacted GlcN. A calibration curve of GlcN was performed in triplicate at 12, 10, 8, 6, 4, 2 µg mL1, and the fluorescence was measured at λexcitation = 340 nm and λemission = 450 nm. Three different batches of USPIO-PAA-GlcN were quantified in order to ensure the reproducibility of the coupling reaction. 3.8.4 In vitro Experiments MSC lines were cultured in IMDM (78%), fetal bovine serum (10%), horse serum (10%), penicillin-streptomycin (1%), and amphotericin-B (1%). Cell passage numbers between 19 and 25 were used. Cell were plated in 6 well-plates, 1.5 × 105 cells/plate and labeled with 100 μg mL1 of IONs for 24 h (n = 6) following the protocol described elsewhere242 with slight modifications. Briefly, MSCs were incubated for 24 h in the presence of IONs (100 µg mL1) or IONs (100 µg mL1) premixed with PLL (1.5 µg mL1, vigorously shaken at 1300 rpm for 1 h). After the cell incubation period, the medium was removed and cells were washed three times with 1.5 mL of PBS (without Mg2+ and Ca2+). After washing, the cells were left for 12 h in 1 mL of fresh label-free medium. Next, the cells were washed once with 1.5 mL of PBS, and 0.5 mL of EDTA-trypsin was added to detach the cells from the well. The detached cells were collected, and after a centrifugation (1000 rpm for 5 min) the supernatant was discarded and the cells were resuspended in fresh medium. Labeled and non-labeled MSCs were plated sequentially to evaluate the possible cellular toxicity and labeling clearance. Characterization of MSCs after labeling was performed at different cellular points: 12 h, and 2, 5, 8 and 12 days after labeling. 3.8.5 Incubation between PLL and USPIO-PAA-GlcN The incubation between PLL (1.5 mg mL1) and USPIO-PAA-GlcN (100 mg mL1) was performed in phosphate buffer at 37 °C for 24 h. The purification of the NPs from unbound PLL was performed by centrifugation (30000 rpm for 30 min), and the pellet
Chapter 3 Stem Cell Labeling 99 was redispersed in water and purified again by centrifugation. NPs from the pellet were dried and analyzed by IR spectroscopy. 3.8.6 ICP of Labeled MSC A total of 1 x 105 cells were dissolved in 1 mL of 37% HCl solution and 4 mL of water was added. The Fe concentration was determined by ICP using an ICPE-9000 Multitype ICP Emission Spectrometer from Shimadzu. Measurements were performed in triplicate and the results are shown as the mean value with the standard deviation. 3.8.7 PB Staining PB staining was performed to demonstrate the uptake of the IONs by the cells. Labeled cells were plated and after 8 h washed with PBS and incubated for 20 min with a mix of equal parts of aqueous solution of HCl (20%) and aqueous solution of potassium ferrocyanide trihydrate (10%). After incubation, cells were washed three times with PBS and images were taken using an inverted microscope. 3.8.8 LDH Assay For assessing the viability of the cells after labeling, supernatants from the incubation between USPIO-PAA-GlcN and MSCs were collected, including a negative control of lysed cells. Cell viability was determined by means of LDH following the manufacturer’s protocol. In brief, supernatants were subjected to centrifugation at 1000 rpm for 5 min and further incubated with LDH reagents for 20 min. Next, the absorbance of the plate was read at 490 nm and the viability rate was calculated with respect to control and lysed values. 3.8.9 Cell Count Total cell count was performed with Trypan blue staining and a Neubauer counting chamber. Samples were diluted 1:5 with PBS and 1:2 with Trypan blue. Cell count was performed using an inverted microscope.
Chapter 3 Stem Cell Labeling 100 3.8.10 In vivo Experiments Experimental animals: all procedures involving the use of research animals were approved by the Research Committee of the University Clinical Hospital of Santiago de Compostela (Spain) and were performed according to the “Principles of Laboratory Animal Care” (NIH publication No. 86-23, revised 1985), as well as specific Spanish (RD 1201/2005 and RD 53/2013) and European Union (Directives 86/609/CEE, 2003/65/CE, 2010/63/EU) regulations. Male Wistar rats (Harlan Laboratories, Barcelona, Spain) weighing 290 ± 10 g were kept in a controlled environment at 22 ± 1 °C and 60 ± 5% humidity, with 12:12 h light: darkness cycles and were fed ad libitum with standard diet pellets and tap water. All surgical procedures and MRI studies were conducted under Sevofluorane anesthesia (3–4%) using a carrier 65:35 gas mixture of N2O: O2. Healthy animals (n = 3) were anesthetized and 2.5 × 105 USPIO-GlcN labeled MSCs suspended in 300 µL of PBS were administered into the brain intra-arterially (perfusion rate: 20 µL/min) through one of the external carotid and with the common carotid opened. 3.8.11 MRI Studies All MRI studies were conducted using a 9.4 T MR system with 440 mT/m gradients and a combination of a linear birdcage resonator (7 cm in diameter) for signal transmission and a 2 × 2 surface coil array for signal detection. A quadrature volume coil (7 cm in diameter) was also used in phantom studies. MRI post-processing was performed using ImageJ software. 3.8.12 Agar Phantoms Agar phantoms were made following a previously described procedure242 with 1 x 105 cells per condition. T2*-weighted and T2-weighted images were acquired 0, 2, 5, 8 and 12 days after the cell plantation.
Chapter 3 Stem Cell Labeling 101 T2*-weighted images were acquired using a multi-gradient echo (MGE) sequence with 4.44 ms echo time, 1.8 s repetition time, 16 echoes with 6.75 ms echo spacing, implemented with a flip angle (FA) of 30º, 14 slices, 2 averages, field of view (FOV) of 7.5 × 7.5 cm2, and a matrix size of 256 × 256. T2-weighted images were acquired using a multi-slice multi-spin-echo sequence (MSME) with 10.44 ms echo time, 3 s repetition time, 16 echoes with 10.4 ms echo spacing, implemented with a FA of 108º, 14 slices, 1 average, FOV of 7.5 × 7.5 cm2, and a matrix size of 256 × 256. 3.8.13 In vivo MRI In order to assess USPIO-GlcN labeled MSCs in vivo, animals were scanned following T2-weighted and T2*-weighted sequences in MRI to evaluate the presence and the distribution of injected cells at 1 h, and 1, 5 and 8 days after the injection. T*2-weighted images were acquired using a MGE sequence with a 2.9 ms echo time, 1.5 s repetition time, 16 echoes with 3.28 ms echo spacing, implemented with a FA of 30°, 14 slices, 2 averages and with a 19.2 × 19.2 mm2 FOV, a 192 × 192 image matrix (isotropic in-plane resolution of 100 μm/pixel × 100 μm/pixel). T2-weighted images were acquired using a MSME sequence with a 9 ms echo time, 3 s repetition time, 16 echoes with 9 ms echo spacing, implemented with a FA of 180°, 2 averages, 14 slices of 1 mm and 19.2 × 19.2 mm2 FOV, a 192 × 192 image matrix (isotropic in-plane resolution of 100 μm/pixel × 100 μm/pixel).
102
Chapter 4 Clickable Iron Oxide Nanoparticles 103 CHAPTER 4 4 Clickable Iron Oxide Nanoparticle: Towards Responsive Controlled Release and Targeting
Chapter 4 Clickable Iron Oxide Nanoparticles 110 4.4 ISOCYANATES FOR ION FUNCTIONALIZATION 4.4.1 Synthesis of Isocyanate Ligands Two different moieties were chosen to decorate the surface of IONs in order to have two possibilities for the functionalization: maleimide and alkyne. The maleimide moiety offers reactivity in the thermally reversible DielsAlder cycloaddition which opens the possibility to induce the release of molecules of interest by heating,55 while also being a substrate for thiolyne click reactions.245 On the other hand, the alkyne moiety enables functionalization with copper-catalyzed alkyneazide cycloaddition (CuAAC), which offers an easy and reproducible way of functionalization with a wide variety of commercially available azides.250 The synthesis of literature-known 4-maleimidophenyl isocyanate251 (5) started with the reaction of 4-aminobenzoic acid (6) and maleic anhydride (7) (Scheme 10). Then, carboxylic acid 8 was dehydrated to form a five-membered ring upon treatment with acetic anhydride (9) under basic conditions. The carboxylic acid in 10 was transformed into acyl chloride 11 using thionyl chloride, and purified by crystallization in a solvent mixture of dried hexane/acetone (1:3). Acyl azide 12 was obtained by the subsequent nucleophilic substitution of the chloride in 11 with sodium azide. In the final step, Curtius rearrangement of acyl azide 12 gave maleimidophenyl isocyanate 5. In summary, 4-maleimidophenyl isocyanate (5) was obtained in five steps with an overall yield of 35%, and all intermediates were obtained without the need of chromatographic purifications. Maleimidophenyl isocyanate 5 was kept under N2 to avoid hydrolysis by atmospheric water.
Chapter 4 Clickable Iron Oxide Nanoparticles 111 Scheme 10: Synthetic route for 4-maleimidophenyl isocyanate (5). Alkyne isocyanate 13 was obtained in three steps starting from 4-hydroxybenzoic acid (14) that was reacted with propargyl bromide (15) to give carboxylic acid 16 (Scheme 11). The conversion of the carboxylic acid in 16 was possible in only one step by the in situ transformation to acyl chloride and the following substitution with sodium azide which afforded the acyl azide 17 in 80% yield.252 The transformation of 17 to alkyne isocyanate 13 was performed by Curtius rearrangement in benzene as a solvent to lower the temperature of the transformation to 80 °C due to the side reactions observed at 110 °C with toluene as solvent. Alkyne isocyanate 13 was successfully synthesized in three steps with an overall yield of 55% and stored under N2 due to its sensitivity against water. Scheme 11: Synthetic route for the alkyne isocyanate 13.
Chapter 4 Clickable Iron Oxide Nanoparticles 112 4.4.2 ION Functionalization with Isocyanates With the ligands in hand, the functionalization of naked IONs was performed with maleimide isocyanate 5, alkyne isocyanate 13, and with an equimolar mixture of isocyanates maleimide 5 and alkyne 13 in order to obtain nanoparticles with two orthogonal groups allowing for the attachment of both drugs and targeting molecules. The first functionalization of IONs with isocyanates was described by Licandro and coworkers,248 and they performed the reaction in toluene at 60 °C under sonication to ensure the dispersion of naked IONs. Therefore, we first investigated the reactions under these conditions (Scheme 12). We found two key factors influencing the success of the nanoparticle functionalization with the isocyanate ligands. First, prior to the functionalization reaction, IONs were dispersed in water and the pH of the solution set to a specific value to determine the degree of protonation of the hydroxyl groups on the IONs, as showed by the -potential measurements discussed earlier (Figure 53). For the reaction with the isocyanate containing molecules to work the most efficiently, it was found that the pH of the solution containing the nanoparticles must be set around 7 before evaporation of the solvent, to avoid free hydroxide ions and to ensure nucleophilicity of the surface. The second key factor is the selection of solvent for the reaction between the NPs and the isocyanate ligands. The reaction between the NPs and the isocyanate ligands was attempted in DMSO. The TGA results showed no increment in the organic material and no bands from the isocyanate ligand were found by IR spectroscopy. A possible explanation for the failure of the reaction could be the Lewis basic character of DMSO. The solvent molecules can coordinate to the ION surface, thus impeding the reaction. For the reaction to work, the NPs were transferred to a solvent with non-Lewis basic character. Therefore, toluene was maintained as the solvent of choice to perform the functionalization. In all cases, the functionalized nanoparticles were purified by centrifugation washing three times with toluene and three times with diethyl ether, and characterized by IR spectroscopy, thermogravimetric assay, elemental analysis, and nuclear magnetic resonance. The characterization of conjugates in the nanoscale is not straightforward;
Chapter 4 Clickable Iron Oxide Nanoparticles 113 therefore, the characterization of Maleimide-Fe3O4 and Alkyne-Fe3O4 was performed first to ensure the success of the functionalization. Scheme 12: Functionalization of naked iron oxide nanoparticles with maleimide isocyanate 5, with alkyne isocyanate 13, and with a 1:1 mixture of maleimide and alkyne isocyanate ligands. The IR spectrum of Maleimide-Fe3O4 (Figure 54) featured vibrational bands at 3300, 1602, and 1240 cm1 corresponding to the stretching peaks of NH, C=O, and CO of the carbamate moiety, respectively. Additionally, the band at 2306 cm1, corresponding to the N=C=O stretching of ligand 5, disappeared after the reaction with the NPs. This suggests the successful reaction between the isocyanate maleimide 5 and the hydroxyl groups on the surface of the IONs. Alkyne-Fe3O4 (Figure 55) showed the characteristics bands at 2900, 1520, 1239, and 571 cm1, corresponding to the stretching of –C≡C–, C=O, CO, and FeO, respectively. At the same time the vibrational band at 2278 cm1, corresponding to the functional group NCO, disappeared after reaction between NPs and ligand 13. This result again suggests the success of the reaction between the hydroxyl groups on IONs and isocyanate 13.
Chapter 4 Clickable Iron Oxide Nanoparticles 114 Figure 54: IR spectrum of maleimide isocyanate 5 (blue), naked Fe3O4 (red), and Maleimide-Fe3O4 (black). Figure 55: IR spectrum of alkyne isocyanate 13 (blue), naked Fe3O4 (red), and Alkyne-Fe3O4 (black). Maleimide-Alkyne-Fe3O4 featured mixed bands from both maleimide and alkyne ligands that were difficult to assign to one particular moiety, with the exception of the strong vibration band at 2900 cm1 due to the stretching of the alkyne moiety (Figure 56).
Chapter 4 Clickable Iron Oxide Nanoparticles 115 Figure 56: IR spectrum of Maleimide-Alkyne-Fe3O4 (green). TGA measurements were performed in order to quantify the amount of organic content in Maleimide-Fe3O4, Alkyne-Fe3O4, and Maleimide-Alkyne-Fe3O4. The results (Figure 57) showed naked Fe3O4 with the lowest organic content as expected, featuring a weight retention of 97 wt%. Maleimide-Fe3O4 showed a weight retention of 51 wt% and Alkyne-Fe3O4 of 63 wt%. On the other hand, Maleimide-Alkyne-Fe3O4 featured the highest organic content with 36 wt%, which may be due to placing the double molar amount of ligands for the reaction mixture. This result is in agreement with the findings of Licandro and coworkers,253 who found the relation of a higher loading of organic material with a higher amount of reacting isocyanate. Both Maleimide-Fe3O4 and Alkyne-Fe3O4 featured two strong weight losses, at 200 and 600 °C for Alkyne-Fe3O4 and at 350 and 700 °C for Maleimide-Fe3O4. Interestingly, Maleimide-Alkyne-Fe3O4 showed at least three strong weight losses at 200, 350, and 700 °C, suggesting the presence of both maleimide and alkyne moieties on the NPs.
Chapter 4 Clickable Iron Oxide Nanoparticles 116 Figure 57: TGA of naked Fe3O4 (red), Alkyne-Fe3O4 (blue), Maleimide-Fe3O4 (black), and Maleimide- Alkyne-Fe3O4 (green). Elemental analysis measurements of the samples (Table 14) were found to be in agreement with the TGA results. Maleimide-Alkyne-Fe3O4 contains the most organic material, followed by Maleimide-Fe3O4 and Alkyne-Fe3O4. Notably, the N% is higher in Maleimide-Fe3O4 when compared to Alkyne-Fe3O4, in agreement with the chemical structure of the maleimide group that contains one additional N atom. The total molar organic content of Maleimide-Fe3O4 is 37.3%, which corresponds to 1.73 mmol of maleimide ligand per g of NP, and is in good agreement with the results of Licandro and coworkers.253 For Alkyne-Fe3O4 the total molar organic content was 31.6%, corresponding to 1.81 mmol of ligand per g of NP. Maleimide-Alkyne-Fe3O4 has two ligands on the surface and it is therefore not possible to calculate the percentage of each ligand by elemental analysis.
Chapter 4 Clickable Iron Oxide Nanoparticles 117 Table 14: Elemental analysis measurements for naked Fe3O4, Maleimide-Fe3O4, Alkyne-Fe3O4, Maleimide-Alkyne-Fe3O4, and the theoretical values for the Maleimide and Alkyne ligands attached to the NPs. Sample % C % H % N Fe3O4 0.054 0.460 - Maleimide-Fe3O4 23.10 1.27 4.28 Maleimide ligand 61.4 3.28 13.02 Alkyne-Fe3O4 18.90 1.86 2.38 Alkyne ligand 68.96 4.63 8.04 Maleimide- Alkyne-Fe3O4 36.06 2.23 6.47 NMR measurements were performed with the three samples to confirm the integrity of the ligands on the nanoparticle. For Maleimide-Fe3O4, the spectrum (Figure 58) featured a singlet at 8.88 ppm corresponding to the NH proton, a pair of doublets in the aromatic region at 7.55 and 7.23 corresponding to the phenyl protons, and a singlet at 7.15 ppm corresponding to the protons of the double bond in the maleimide moiety. These data are in agreement with the work of Licandro and coworkers.253 On the other hand, the proton spectrum of Alkyne-Fe3O4 (Figure 59) featured a peak at 8.45 ppm corresponding to the NH proton, a pair of broad signals at 7.37 and 6.91 ppm corresponding to the phenyl protons, and a singlet at 4.74 corresponding to the CH2 in α-position to the alkyne. Notably, for both samples, the presence of the NH proton indicates the formation of the carbamate on the NP surface. The 1H NMR spectrum of Maleimide-Alkyne-Fe3O4 (Figure 60) featured the proton signals with the same chemical shifts as those for pure Maleimide- and Alkyne-Fe3O4 samples, but the signals corresponding to NH were found as duplicate. This could be the result of the formation of dimers on the NP surface: homodimers would contribute one NH signal each, whereas heterodimers of would result in two additional NH signals. However, more studies would be necessary to prove the dimer formation.
Chapter 4 Clickable Iron Oxide Nanoparticles 118 Figure 58: 1H NMR spectrum (500 MHz, DMSO) of Maleimide-Fe3O4. Figure 59: 1H NMR spectrum (500 MHz, DMSO) of Alkyne-Fe3O4.
Chapter 4 Clickable Iron Oxide Nanoparticles 119 Figure 60: 1H NMR spectrum (500 MHz, DMSO) of Maleimide-Alkyne-Fe3O4. In summary, the reaction between the NPs and maleimide isocyanate 5, alkyne isocyanate 13, and their molar mixture took place, as confirmed by IR spectroscopy, TGA, elemental analysis, and NMR. The efficiency of the reaction could not be calculated, as it was not possible to quantify the hydroxyl groups available in the surface of naked IONs. 4.4.3 Model Reactions In order to find appropriate reaction conditions for the functionalization of the maleimide and alkyne moieties on the surface of IONs, both DielsAlder and CuAAC reactions were studied first in the absence of magnetic nanoparticles to facilitate characterization procedures. The DielsAlder reaction has been known for over 50 years in the literature.254 The diene and dienophile can be tuned to form a cyclized product able to undergo a retrocyclization, which results in a reversible reaction.56 DielsAlder reaction has the desirable characteristic to be self-contained, i.e. all the atoms present in the diene and dienophile are kept in the resulting products, meaning that the displacement of the equilibrium is governed by temperature, solvent, or reactant concentration, but not by outsider molecules such as water, metal catalyst, or base/acid.56
Chapter 4 Clickable Iron Oxide Nanoparticles 126 Figure 64: TGA measurements of naked Fe3O4 (red), Alkyne-Fe3O4 (blue) and Biotin-Alkyne-Fe3O4 (black). Figure 65: Calibration curve of Biotin with HABA-Avidin commercial kit. The DielsAlder reaction was also studied with pure Maleimide-Fe3O4. The reaction conditions selected to functionalize the IONs employed the lower temperature of 65 °C instead of 110 °C used in the model reactions in order to avoid a detachment of the alkyne carbamates from the ION surface. A reaction time of 24 h at 65 °C did not lead to an increase in the organic content of the resulting IONs compared to
Chapter 4 Clickable Iron Oxide Nanoparticles 127 Maleimide-Fe3O4 as shown by TGA, suggesting that DielsAlder reaction did not take place. Therefore, a longer reaction time of 3 days was employed. In this case, TGA measurements showed an increase in the organic content of 9 wt% (Figure 66), indicating that Pyrene-Maleimide-Fe3O4 was obtained successfully (Scheme 17). The UV-Vis spectrum of the resulting IONs in ethanol featured the bands characteristic of furfuryl pyrene 23 at 342, 326, and 267 nm (Figure 67). The thermal release of furfuryl pyrene 23 from Pyrene-Maleimide-Fe3O4 was not tested because the NPs were only dispersable in organic solvents such as THF or ethanol, and thus the testing conditions would not mimic the scenario of physiological conditions. Scheme 17: Diels Alder reaction between Maleimide-Fe3O4 and furfuryl pyrene 23 in toluene at 65 °C for 3 days to yield Pyrene-Maleimide-Fe3O4. After the optimization of the individual reactions with maleimide and alkyne moieties, the doubly functionalized NPs Maleimide-Alkyne-Fe3O4 were tested. The DielsAlder reaction was selected to be the first to ensure the steric availability of the maleimide moieties.
Chapter 4 Clickable Iron Oxide Nanoparticles 128 Figure 66: TGA measurements of naked Fe3O4 (red), Maleimide-Fe3O4 (blue) and Pyrene- Maleimide-Fe3O4 (black). Figure 67: UV-Vis spectrum of Maleimide-Fe3O4, furfuryl pyrene 23, and Pyrene-Maleimide-Fe3O4 in ethanol.
Chapter 4 Clickable Iron Oxide Nanoparticles 129 DielsAlder reaction between the maleimide moiety of Maleimide-Alkyne-Fe3O4 and furfuryl pyrene 23 was conducted over three days at 65 °C in toluene to yield nanoparticles Pyrene-Alkyne-Fe3O4 (Scheme 18). After purification of the nanoparticles by magnetic separation, the CuAAC between the alkyne moiety of the nanoparticles and the commercially available N3-PEG-Biotin was performed under the same conditions as for Alkyne-Fe3O4. The purification of Pyrene-Biotin-Fe3O4 was performed by dialysis since the NPs showed good solubility in water after the addition of the PEG linker, as desired for biomedical applications. The characterization of Pyrene-Biotin-Fe3O4 was performed by fluorescence, and the presence of pyrene 23 was verified by the characteristic emission bands of pyrene furfuryl at 416, 394, and 375 nm (Figure 68). Additionally, the presence of the biotin moiety was verified by the HABA-Avidin assay, and Pyrene-Biotin-Fe3O4 was found to bear 7.54 µM of the biotin ligand per g of NP. Characterization by TGA was not possible because of the low quantities of Pyrene-Biotin-Fe3O4 obtained. With the IONs bearing biotin moieties for targeting, pyrene units as model system for drug release, and PEG linkers for water solubility, the thermally controlled release was tested by hyperthermia. Pyrene-Biotin-Fe3O4 was treated for 1 h in water at 200 G in a hyperthermia experiment, then the NPs were collected and washed by centrifugation. The collected washes were analyzed by fluorescence and did not show the characteristics bands of furfuryl pyrene 23, suggesting that the release of the fluorophore did not occur. The reason may be related with a small heat production on the surface of the NPs, probably due to their small core size, which is too low to promote the retro-DielsAlder reaction. The future work will be to employ naked iron oxide NPs with a larger core size (1520 nm) for the functionalization in order to increase the heat production to allow for the release to happen during hyperthermia treatment.
Chapter 4 Clickable Iron Oxide Nanoparticles 130 Scheme 18: Double functionalization of Maleimide-Alkyne-Fe3O4 nanoparticles first with furfuryl pyrene 23 and then N3-PEG-Biotin. Figure 68: Fluorescence spectrum of Pyrene-Alkyne-Fe3O4 in H2O with λexc at 300 nm. On the contrary, preliminary results regarding the thermally controlled release of furfuryl pyrene 23 from Pyrene-Biotin-Fe3O4 were obtained by heating the sample in water for 1 h in an oil bath at 60 °C. After heating, nanoparticles were purified by centrifugation and the supernatant analyzed by fluorescence spectroscopy to evaluate
Chapter 4 Clickable Iron Oxide Nanoparticles 131 the release of pyrene furfuryl 23. The fluorescence results were subtracted from control (non-heated Pyrene-Biotin-Fe3O4 in water). The obtained spectrum (Figure 69) showed the characteristic bands of furfuryl pyrene 23, indicating that the release of the fluorophore by heating was successful. Figure 69: Fluorescence spectrum of the supernatant of Pyrene-Biotin-Fe3O4 after oil bath heating for 1 h at 60 °C in water. 4.6 CONCLUSIONS The functionalization of IONs was tested with two approaches: the functionalization of the Fe precursor, and the functionalization of the synthesized IONs. The first approach failed at the preservation of the organic functional groups on the NP surface after the formation of the nanoparticles. On the other hand, the functionalization of the surface of IONs was possible upon reaction between the hydroxyl groups on the NP surface and isocyanate ligands. The integrity of the functional groups on the IONs was confirmed by infrared spectroscopy, thermogravimetric assay, and nuclear magnetic resonance. Two isocyanate molecules were synthesized bearing alkyne and maleimide moieties. Alkyne functional groups were selected in order to obtain IONs susceptible to react through the well-known copper-catalyzed alkyneazide cycloaddition. The maleimide functional group was selected because it is a substrate of 1,3-DielsAlder reaction,
Chapter 4 Clickable Iron Oxide Nanoparticles 132 which is known to be thermally reversible. The reactivity of IONs functionalized with alkyne and maleimide moieties was confirmed for both in the copper-catalyzed alkyne-azide and the DielAlder cycloadditions. This strategy gave access to IONs functionalized with biotin moieties for targeting, polyethylene glycol linkers for water solubility, and with fluorophore molecules as a model system for a drug. The thermally controlled release was tested with the fluorophore molecules bound to the IONs by the DielsAlder reaction. The liberation of the fluorophore molecules failed by magnetic hyperthermia, while being successful by heating in an oil bath. These results suggest the low heat production by the IONs, and therefore future work will be focused on the production of IONs with higher saturation magnetization and coercivity forces.
Chapter 4 Clickable Iron Oxide Nanoparticles 133 4.7 EXPERIMENTAL Commercially available chemicals were used without further purification. Column chromatography (CC) was carried out with SiO2 (60 Å, 40–63 µm, 230– 400 mesh, Macherey Nagel). Thin-layer chromatography (TLC) was conducted using ALUGRAM Xtra SIL G UV254 aluminium sheets from Macherey Nagel, and visualized by exposure to ultraviolet light. Dried solvents (DMF, DMA, toluene, acetone, MeCN, and MeOH) for reaction and crystallization procedures were purchased from Acros Organics in Extra Dry over 4 Å molecular sieves quality with less than 0.5% of H2O. Mass spectrometry (MS) experiments were performed on a Bruker APEX® III FTMS (ESI) and Waters Micromass GC-TOF (EI) instruments at Centro de Apoio Científico e Tecnolóxico á Investigación (C.A.C.T.I.) at the University of Vigo, Spain. Proton nuclear magnetic resonance (1H NMR) spectra of organic compounds were recorded on a 400 MHz Bruker Avance II spectrometer at the NMR service of University of Minho in Braga, Portugal. For iron oxide nanoparticles spectra was recorded on a 500 MHz Bruker DRX-500 and 300 MHz Varian Mercury 300 Robot at the NMR service of Universidade de Santiago de Compostela, Spain. Proton chemical shifts are expressed in parts per million (δ scale) and are calibrated using residual undeuterated solvent peaks as an internal reference (CDCl3: δ 7.26; (CD3)2SO: 2.50). Data for 1H NMR spectra are reported as follows: chemical shift (δ ppm) (multiplicity, coupling constant (Hz), integration). Multiplicities are reported as follows: s = singlet, d = doublet, t = triplet, q = quartet, m = multiplet, br = broad. Carbon nuclear magnetic resonance (13C NMR) spectra were recorded on a 400 MHz Bruker Avance II spectrometer. Carbon chemical shifts are expressed in parts per million (δ scale) and are referenced to the carbon resonances of the solvent (CDCl3: δ 77.16; (CD3)2SO: δ 39.52). Fourier transform infrared spectroscopy (IR) spectra were acquired on a Bruker VERTEX 80v FT-IR spectrometer in absorbance mode. A spatula tip of the sample was
Chapter 4 Clickable Iron Oxide Nanoparticles 134 mixed with 200 mg of KBr and the powder was pressed at 10 tons for 2 min to obtain a transparent pellet. Spectra were recorded at 1.66 hPa with 32 scans and 4 cm1 resolution with deuterated triglycine sulfate detector. The empty holder at 1.66 hPa was used as background and baseline correction was applied to the spectra. TGA was performed in a TGA/DSC 1 STARe system, Mettler-Toledo, fitted with OmniStar GSD320 gas analysis system (Pfeiffer Vacuum), with 10 K min1 gradient from 30 to 900 °C under 30 mL min1 of Ar flow. UV-Vis and fluorescence spectroscopy were carried out at room temperature with 1 cm path-length Hellma quartz 111-QS cuvettes. UV-vis spectra were recorded with a Shimadzu UV-2550 spectrophotometer. Fluorescence spectra were recorded with Horiba Fluoromax-4 spectrofluorometer. Elemental analysis were performed on Elemental Carlo Erba 1108/Combustion chromatography system at the service of C.A.C.T.I. at the University of Vigo, Spain. Absorbance for HABA/avidin bioassay was measured with BioTek, Synergy H1 hybrid reader at 500 nm. Standard calibration curve was done with HABA/avidin and biotin standard solution in buffer from Sigma Aldrich (0 to 12 µM). TEM studies were performed using Titan ChemiSTEM (FEI, 0.08 nm STEM resolution) electron microscope, operated at 200 kV and equipped with a Super-X detector.
Chapter 4 Clickable Iron Oxide Nanoparticles 135 4.7.1 Synthetic Procedures 3-Allylacetylacetonate246 (1) Na2CO3 (3.3 g, 24 mmol) was added to a 1 M solution of acetyl acetone (1) (2.0 g, 20 mmol) in anhydrous acetone under N2, and left to stir for 30 min at rt. Allyl iodine (2) (2.2 mL, 24 mmol) was added dropwise, and the mixture was stirred 12 h at 56 °C. The reaction mixture was filtrated, and the filtrate was evaporated in vacuo. Purification by CC (SiO2; hexane/EtOAc 40:1) gave 3 (1.6 g, 48%) as yellow oil and a mixture of tautomers. 1H NMR (400 MHz, CDCl3): 16.62 (s, 1Hb’), 5.805.70 (m, 1Hd’), 5.655.56 (m, 1Hd), 5.024.88 (m, 4He,e’), 3.65 (t, J= 6.4 Hz, 1Hb), 2.912.89 (m, 2Hc’), 2.512.47 (m, 2Hc), 2.09 (s, 6Ha), 2.07 (s, 6Ha´). 13C NMR (100 MHz, CDCl3): 203.3, 191.2, 135.5, 133.9, 117.1, 114.5, 106.8, 67.4, 31.9, 30.8, 29.0, 22.5. EI-MS: m/z (%): 140.08 (12, [M]+, calcd for C8H12O2+ = 140.0837), 97.06 (100, calcd for C6H9O+ = 97.0654), 83.05 (48), 98.07 (42). Iron(III) 3-Allylacetylacetonate247 (4) A solution of 3 (1.7 g, 12.5 mmol) in MeOH (2.5 mL, 5 M) was added dropwise to 0.1 M aq solution of FeCl3 •6H20 (1.3 g, 4.7 mmol). The color of the reaction mixture changed from yellow to black, and then an aq. solution of sodium acetate (NaOAc) (3.8 mL,