Full text
Food Packaging and Shelf Life 42 (2024) 101264 Available online 1 March 2024 2214-2894/© 2024 The Author(s). Published by Elsevier Ltd. This is an open access article under the CC BY license (http://creativecommons.org/licenses/by/4.0/). Innovative films by embedding magnetic nanoparticles in cellulose acetate Lisandra de Castro Alves a , * , Miguel A. Cerqueira b , * , Manuel A. Gonz´ alez-Gom´ ez a , c , Pelayo Garcia-Acevedo a , ´ Angela Arnosa Prieto a , Yolanda Pi˜ neiro Redondo a , Lorenzo Pastrana b , Jos´ e Rivas a a Nanotechnology and Magnetism Lab — NANOMAG, Materials Institute – iMATUS, Health Research Institute – IDIS, Department of Applied Physics, Universidad de Santiago de Compostela, E-15782 Santiago de Compostela, Spain b Food Processing and Nutrition Group, International Iberian Nanotechnology Laboratory-INL, Av. Mestre Jos´ e Veiga s/n, 4715-330 Braga, Portugal c Nanostructured Materials Group, International Iberian Nanotechnology Laboratory-INL, Av. Mestre Jos´ e Veiga s/n, 4715–330 Braga, Portugal ARTICLE INFO Keywords: Biopolymer Film Magnetism Smart packaging Nanoparticle Anti-counterfeiting ABSTRACT Magnetic nanoparticles (MNPs) with different magnetic, physical, and chemical properties can be used to develop magnetic tags, offering a unique traceability capability that can then be used to improve products’ safety. In this work, synthesized MNPs were incorporated into a cellulose acetate (CA) matrix and characterized in their pristine form and when incorporated in the films. Results show that MNPs are different in composition, morphology, size, and magnetic response. Afterwards, iron carbide (Fe 5 C 2 ), hexagonal-shaped (Fe 3 O 4 @OA) and multicore magnetite (m-Fe 3 O 4 ) nanoparticles (NPs) were embedded within the CA matrix showing and good distribution in the films’ matrix. Nevertheless, magnetic films with 0.1 wt% of Fe 5 C 2 NPs (FM1), and m-Fe 3 O 4 NPs (FM4) offered a more uniform dispersion of the NPs over the CA matrix. Incorporating MNPs does not affect the films’ mechanical properties and water sensitivity. Nevertheless, the optical properties of the films were affected with high impact for the films with m-Fe 3 O 4 NPs. Particularly for magnetic tagging, the CA films displayed similar magnetic responses to their respective bulk NPs, showing their potential as anti-counterfeiting tags for food packaging applications. 1. Introduction The impact of counterfeiting industrial products reaches not only the economic sphere but also the social one since counterfeit objects lack the guarantees and quality control of authentic products. Counterfeiting reaches the entire production chain from raw materials to spare parts and products for a wide variety of sectors, such as documents or paper currency, drugs, cosmetics, food, clothing, etc (Ghadge et al., 2021). The majority of used anti-counterfeiting strategies rely on smart packaging methods that incorporate fluorescent materials like organic dyes, lanthanide-based materials, and carbon dots (CDs). These materials are utilized employed to create security features such as barcodes, holograms, watermarks, or colored fibers, which enhance security but provide only a basic level of protection. For this reason, there is a need for more innovative and cost-effective anticounterfeiting techniques that provide superior multi-level security features capable of encoding data for large-scale trade management (Leng et al., 2017; Liu et al., 2019; Miao et al., 2018; Muthamma & Sunil, 2022; You et al., 2016). A strong effort is driving research towards developing new packaging materials with smart properties using non-petroleum-based polymers. On this behalf, biopolymers are gaining popularity due to their worldwide availability, sustainability, biocompatibility, and versability, whether are derived from animal or vegetal origin (Raghuvanshi et al., 2023). Polysaccharides are carbohydrates synthesized by plants, animals, and humans, consisting of glucose as the monosaccharide unit (L. Yang et al., 2022). Most natural polysaccharides, namely chitosan, gelatin, and cellulose, have been reported as binders in security inks, films, paper, and anti-counterfeiting composites (L. Yang et al., 2022). Cellulose, one of the most abundant natural polysaccharides, stands out for its cost-effectiveness, making it attractive for practical applications, especially in food packaging (Soon & Manning, 2019) and anti-counterfeiting (Campos-Cuerva et al., 2016). Recently, cellulose films containing LiCl crystals on their surface have been developed to control solution viscosity and temperature. The final film exhibits * Corresponding authors. E-mail addresses: [email protected] (L. de Castro Alves), [email protected] (M.A. Cerqueira). Contents lists available at ScienceDirect Food Packaging and Shelf Life journal homepage: www.elsevier.com/locate/fpsl https://doi.org/10.1016/j.fpsl.2024.101264 Received 10 October 2023; Received in revised form 25 January 2024; Accepted 25 February 2024
Food Packaging and Shelf Life 42 (2024) 101264 2 excellent mechanical strength, hydrophilic properties, good thermal resistance, and great potential for anti-counterfeiting purposes (Jing et al., 2022). Other examples were presented using cellulose nanocrystal-based liquid crystal structures (Wei et al., 2021) and by functionalizing cellulose fibers with lanthanide-based luminescent core/shell nanoparticles (Szczeszak et al., 2022). Among, cellulose derivatives, cellulose acetate is widely used in packaging leading to the creation of biodegradable films (Teixeira et al., 2021; Yuan et al., 2022; Zhou et al., 2022) its use in developing anti-counterfeiting has been mostly focused on forming fibers, and coatings with the incorporation of luminescent compounds (Chen et al., 2021; Hendrick et al., 2010; Jin et al., 2023; Mogharbel et al., 2023). Another possible strategy to develop materials with unique features for anti-counterfeiting purposes is by incorporating small magnetic nanoparticles (MNPs), with superparamagnetic behavior. They can impart a magnetic signal to the hybrid material that can be used for detection purposes. Although different MNPs, such as SmCo 5 (Radojevic et al., 2004) or PbS (Lu et al., 2005) NPs, can be used to provide enhanced magnetic response, the MNPs are more competitive due to their cost-effectiveness and scalable production methods. In addition, the small size of the MNPs allows for uniform distribution within the biopolymer, minimizing the impact on physicochemical properties when appropriate nanoparticles functionalization is used to ensure chemical compatibility between inorganic and organic matrices (Robertson & Nyy, 2014). In this regard, some studies have shown the compatibility of MNPs in different biopolymer-based matrixes such as chitosan and pectin (Farjadian et al., 2017; Surendhiran et al., 2022; Zarandona et al., 2023), starch (Keshk et al., 2019), gelatin (Mehmood et al., 2020), poly(3-hydroxybutyrate-co-3-hydroxyvalerate (PHBV) (Abdalkarim et al., 2020). Some studies also showed that incorporating customized MNPs into cellulose acetate increases the thermal stability of films (Jalajerdi et al., 2012) and can provide counterfeit identification abilities (Robertson & Nyy, 2014). for tagging products. This shows that limited efforts have been made to develop cellulose acetate films incorporating MNPs as magnetic tags for product authentication and counterfeit identification. Therefore, this study explores the incorporation of different MNPs into a cellulose acetate matrix to produce magnetic films with varying magnetic properties for tagging applications. The tagged cellulose acetate films include cellulose acetate, a plasticizer, and different MNPs. MNPs with different compositions, morphology, size, and magnetic response were prepared, such as iron carbide (Fe 5 C 2 ), hexagonal and multicore-Fe 3 O 4 nanoparticles (NPs) that were fully characterized. 2. Material and methods 2.1. Materials All the chemicals were of analytical grade and were used as received without further purification. Octadecylamine (98%), cetrimonium bromide (CTAB, 98%), oleylamine (OA, 70%), iron (III) acetylacetonate (Fe (acac) 3 , 99%), iron (III) chloride hexahydrate (FeCl 3 .6 H 2 O, 99%), absolute ethanol, acetone, toluene, hexane (95%), oleic acid (OA, 90%), polyvinylpyrrolidone (MW 40.000), sodium acetate anhydrous (NaAc >99%), cellulose acetate (Mn 50.000 Da), triethylamine (TEA, 99%), benzyl ether (98%) was acquired from Sigma Aldrich. Chloroform (99%) from Prolabo, pyromellitic dianhydride (PMDA ≥97%) from Alfa Aesar, ethylene glycol (95%) from Fluka and iron pentacarbonyl (Fe(CO) 5 C 2 ) from Acros organics. 2.2. Synthesis of iron carbide (Fe 5 C 2 ), hexagonal-shaped (h-Fe 3 O 4 ), and multicore magnetite (m-Fe 3 O 4 ) NPs Fe 5 C 2 NPs were prepared according to the method described elsewhere (G. Huang et al., 2014). Briefly, 7.0 g of octadecylamine, 0.8 g of CTAB, and 2 mL of OA were mechanically stirred and heated to 180 ◦C under Argon flow. Afterwards, 0.2 mL of Fe(CO) 5 C 2 (1.5 mmol) was added. The reaction was left agitating for 10 min at 180 ◦C, and then the temperature increased to 350 ◦C and was kept agitating for 30 min (M1). It was kept agitating for 60 min (M2) in another procedure. Both solutions were left to cool down and washed with ethanol and hexane to remove any octadecylamine excess. The Fe 5 C 2 NPs, were labeled as M1 and M2 and redispersed in hexane until further use. Hexagonal NPs coated with oleic acid (h-Fe 3 O 4 ) were also prepared following the method described (Kim et al., 2009). Briefly, 0.7 g of Fe (acac) 3 was added to a previous mixture of 1.10 g and 10.4 g of OA and benzyl ether, respectively. The solution was mechanically stirred for 1 h at 25 ◦C and then at 300 ◦C for 30 min. After cooling, a previously prepared solution of toluene and hexane was added, to precipitate the hexagonal shaped Fe 3 O 4 , which was labeled as M3. NPs were washed by centrifugation using chloroform. Lastly, the multicore magnetite (m- Fe 3 O 4 ) NPs were prepared by the solvothermal method, as described in other work (Zhu & Diao, 2011) with minor modifications. It was added, 1.5 g FeCl 3 .6 H 2 O, 1.0 g polyvinylpyrrolidone (PVP 40), and 2.0 g of NaAc to 30 mL ethylene glycol. The mixture was stirred for 2 h and autoclaved for 8 h at 200 ◦C. The product solution was cleaned with ethanol, and the synthesized m-Fe 3 O 4 NPs were dried at 60 ºC previously to their use. These NPs were named M4. 2.3. Magnetic films preparation The magnetic cellulose acetate (CA) films were prepared by the (Kaschuk et al., 2021) anhydride groups and the hydroxyl groups in CA. Firstly, 8.0 g of CA was added to 100 mL of acetone. Then, 0.4 g of PMDA cross-linker was added to 40 mL of the previously prepared CA solution. At this stage, the agitation speed was increased (500 rpm) for a faster PMDA dissolution, and once the mixture has been homogenized, the rate is decreased (150 rpm) to avoid the formation of air bubbles. CA solutions were prepared with MNPs (Fe 5 C 2 , h- Fe 3 O 4 , and m-Fe 3 O 4 ) concentrations ranging from 0.02 to 0.2 wt%. After complete dissolution and dispersion of NPs, 20 µL of TEA catalyst was added to each solution and stirred for 1–2 min. To produce the films, 20 mL of this forming was cast onto a Petri dish (D 1 =13.5 cm and D 2 =9 cm), and dried initially at room temperature for 48 h. Films were peeled off from the Petri dish, and stored at room temperature inside a desiccator with 54% relative humidity (RH). Saturated salt solution of Mg(NO 3 ) 2 was used to achieve this RH. 2.4. Films and nanoparticles characterization 2.4.1. X-ray diffraction (XRD) and fourier-transform infrared (FTIR) spectroscopy The X-ray diffractometer Philips type powder fitted with PW1710 control unit, PW1820/00 (PANalytical, Almelo, Netherlands) was used for XRD analysis. The crystal structure of both nanoparticles and magnetic films were determined with a Cu K α (40 kV, 30 mA) radiation operating at a step size of 0.02◦and counting time of 2 s per step over a 2θ range of 2–40◦at room temperature. FTIR spectra were recorded using a Varian FT-IR 670 spectrophotometer (Agilent Technologies, Santa Clara, CA, USA). The scanning range was 4000–400 cm −1 with 64 scans and a resolution of 4 cm −1 . 2.4.2. Transmission electron microscopy (TEM) and scanning electron microscopy (SEM) The morphology of the MNPs was analysed using a JEOL JEM-1011 microscope (JEOL, Tokyo, Japan) operating at 100 kV. Previously to the measurements a diluted solution of each particle was prepared. A drop of the diluted particle solution (approximately 10 µL) was deposited onto a copper grid with a thin layer of carbon film (Formvar films) and was left to dry under a white light bulb. The surface morphology of the CA films was examined using a SEM ZEISS EVO LS15 microscope (Zeiss, L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 3 Oberkochen, Germany) operating at 20 kV. Previously to the measurements, the samples were assembled onto aluminums stubs using conductive double-sided adhesive carbon tabs (Pro SciTech). 2.4.3. Mean particle size, polydispersity index (PDI) and zeta potential The mean particle size, PDI and zeta potential were performed with at least 3 replicates at 25 ◦C using a NanoZS (Malvern Instruments, Malvern, UK) with an angle detection of 173◦. 2.4.4. Thermogravimetric analysis (TGA) TGA was recorded using a Perkin Elmer TGA 8000 (Perkin, Waltham, MA, USA) with a flow rate of 20 ◦C/min and a heating rate of 25 ◦C/min (temperature range 50 to 850 ◦C) under oxygen atmosphere. 2.4.5. Vibrating-sample magnetometer (VSM) The magnetic properties of the sample were evaluated by measuring the magnetization hysteresis loops using a vibrating sample magnetometer (VSM) from DMS, located in Massachusetts, USA. The VSM was operated at room temperature with an applied field ranging from −10,000–10,000 Oe. 2.4.6. Confocal Raman microscopy The Raman spectra was obtained from an WITec Raman confocal microscope (model=ALPHA300R+) with a Zeiss 50x Epiplan-Neofluar objective (Oxford instruments, Ulm, Germany) and the film samples were measured using an excitation of 0.3 s integration and 450 scans. 2.4.7. Profilometry The confocal laser optical profilometry results were obtained with a 3D Optical Profiler (Sensofar S. Neox, Terrassa, Spain) microscope with a white-light vertical scanning interferometry (VSI) mode and CFI60–2 Nikon objective lens. The topography images of the CA films were obtained using objective lenses of 10x and 20x and the images were processed using the SensoMap software. The following roughness parameters were obtained, Root mean square (Rq,µm), total height of profile (Rt,µm)skewness (Rsk,µm),and kurtosis (Rku,µm). The parameters were calculated by the instrument from multiple measures in each area [20]. 2.4.8. Atomic force microscopy (AFM) The surface morphology of the films was analyzed using an XE-100 (Park Systems Corporation) AFM equipment working in a non-contact mode (NC-AFM). One film was analyzed per composition. 2.4.9. Mechanical properties Mechanical properties of the films were measured using a Shimadzu AGX-V (Shimadzu Corporation, Kyoto, Japan) with a load cell of 500 N and an elongation rate of 50 mm/min. It was prepared with at least 4 replicates per film sample with 2 ×7 cm. The thickness of the films was recorded using an electronic micrometer (Schutt, graduation 0.001 mm). As a result, the tensile stress, σ ( ε ), was calculated by dividing the maximum force to rupture, F( ε ),by the cross-section area, A0, of the films. The result is expressed in megapascals (MPa), and the Eq. (1) is as follows (Cook, 1984): σ ( ε ) = F( ε ) A0 (1) The strain, ε , is related to the microfiber length and was calculated using Eq. (2): ε (t) = L(t) − L0 L0 (2) Where, L0, is the original length of the material and L,is the length of the material at time t.The strain result is usually presented in percentage for better representation (since is a ratio of lengths, strain has no units). Young’s modulus, E, evaluates the elasticity of a material and the capacity to resist deformation. E, and was calculated from the slope of the elastic region according to Eq. (3). A higher Youngs´s modulus is correlated to a higher resistance of the material against deformation (Fourne, 1999): E=Δ σ ε Δ ε (3) 2.5. Moisture content and water solubility The sensitivity of the films to water was analyzed through the determination of moisture content (MC) and water solubility. MC of the films was determined following the method described elsewhere (Costa et al., 2015). Briefly, five replicates of approximately 50 mg of each film were cut and stored at 25 ◦C at a relative humidity of 65% for 24 h. Afterwards, the films were weighted, posteriorly dried at 105 ◦C for 24 h, and finally weighted to calculate MC using the following Eq. (4): Moisture content (%) = (Mi−Mf Mi)∗100 (4) where, Mi and Mf are the masses of initial (before dried) and dried films (mg), respectively. Afterward, it was tested the solubility of the film pieces by analysing the content of dry matter solubilized after 24 h of immersion in water at approximately 20 ºC. The percentage of water solubility of the films was calculated following the Eq. (5): Solubility (%) = (Si−Sf Si)∗100 (5) where, Si is the initial weight before solubility (mg), and Sf is the dry matter (mg) that was not solubilized in water after the film pieces were dried at 105 ◦C for 24 h. 2.5.1. Opacity and color The CIElab scale was used to determine the colour parameters (L*, a*, b*). In this sense, L* indicates the lightness (which ranges from black to white) and a* (reveals the difference in green (-a*) and red (+a*)) and b* (difference between blue (-b*) and yellow (+b*)) are the chromatic parameters (Ly et al., 2020). The colour parameters were obtained by using a Minolta colorimeter in three replicates of each film. The films were superposed on a white standard background, and a set of colour coordinates were given for each replicate. The total difference value (ΔE) was determined following the Eq. (6): ΔE=(ΔL2+Δa2+Δb2)0.5(6) where, ΔL=Lstandard −Lsample; Δa=astandard −asample; Δb=bstandard −bsample.The standard values used were the ones from the control films. The opacity percentage was also determined according to the Hunterlab method (Cheng et al., 2018), following the Eq. (7): Opacity (%) = Yb Yw ∗100 (7) Where, Y is the CIE tristimulus value of the film on a black standard (Yb) and on a white standard (Yw). It was taken three measurements per film. 2.5.2. Statistical analysis Statistical analysis was performed using one-way ANOVA with a 99% confidence level using Vassarstats (http://vassarstats.net). L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 4 3. Results and discussion 3.1. Nanoparticles characterization 3.1.1. Morphological observation TEM was used to precisely determine the size and morphological structure of the synthesized nanoparticles, enabling a comprehensive evaluation of their physical properties. The TEM images and respective size histograms of the synthesized MNPs are shown in Fig. 1. Fe 5 C 2 NPs with different mean sizes are presented in Fig. 1a (M1) and 1b (M2), and Fe 3 O 4 NPs with hexagonal (M3) and multicore configuration (M4) in Fig. 1c and d, respectively. The magnetic Fe 5 C 2 (M1) NPs have a heterogenous morphology and a size distribution of 21 nm. Meanwhile, the Fe 5 C 2 (M2), have a mean diameter of 77 nm and a more homogenous morphology with sphericallike shape that can be explained by the longer reaction time during synthesis (G. Huang et al., 2014). TEM image (Fig. 1c) revealed a hexagonal like-structure of the as-synthesized Fe 3 O 4 (M3) NPs with a uniform size diameter of 145 nm. TEM image (Fig. 1d) of the multicore-Fe 3 O 4 (M4) NPs revealed that each nanoparticle consists of many magnetic cores with a final spherical structure and size diameter of approximately 292 nm. 3.1.2. Structural and textural characterization XRD and FTIR techniques were selected to provide valuable insights into the composition, crystal structure, and surface properties of the synthesized NPs. The infrared spectra and diffractograms are shown in Fig. 2a and b, respectively. The FTIR spectra of both Fe 5 C 2 NPs (M1 and M2) in Fig. 2a, reveal distinctive adsorption bands at 2846 and 2938 cm −1 , attributed to the asymmetric and symmetric stretch vibrations, - CH 2 , respectively. These peaks are characteristic of Fe 5 C 2 NPs. Furthermore, there are observable adsorption bands corresponding to Fe-O at 558 cm −1 , and 633 cm −1 which is typical associated with Fe 3 O 4 and γ-Fe 2 O 3 (Parikh et al., 2014; Xuan et al., 2007). This observation strongly supports that Fe 5 C 2 is not the only magnetic phase present in the sample. Besides this, in the spectra of M3 and M4 NPs is also present at 558 cm −1 the band of Fe-O corresponding to Fe 3 O 4 but in a more pronounced way. A comparison of the diffraction patterns between Fe 3 O 4 (M3 and M4) and Fe 5 C 2 NPs (M1 and M2) are shown in Fig. 2b. The XRD diffractogram of Fe 5 C 2 NPs (M1 and M2) revealed distinct diffraction peaks located at 2Ө=35.4, 39.3, 43.2, 44.7, 49.1, 53.2, and 56.1◦, which can be indexed to the (002), (112), (021), (510), (31.2), (402), and (222) planes, respectively. The crystalline structure of M1 and M2 NPs is in alignment with that of Fe 5 C 2 NPs (ICDD: 98–004-3194) (Liu et al., 2020). Conversely, the XRD pattern of both h-Fe 3 O 4 (M3) and m-Fe 3 O 4 (M4) NPs exhibits diffraction peaks located at 2Ө=18.3, 30.1, 35.6, 43, 53.7, 57.2, 62.7, and 74.2◦, corresponding to the (111), (220), (311), (400), (442), (511), (440), and (622) planes of Fe 3 O 4 with a face-centered cubic structure (ICDD: 98–015-8743), respectively. 3.2. CA films characterization 3.2.1. Films surface appearance and MNPs dispersibility The surface morphology of the films was observed by SEM to study their topography, texture, and overall surface structure, including features such as pores, cracks, or irregularities in MNPs dispersibility. The synthesized NPs were incorporated into a cellulose acetate matrix in different amounts, and homogeneously distributed within the hybrid films. Morphological observations of a selected set of magnetic films, and a CA control film are shown in Fig. 3. Generally, the MNPs appear as agglomerates onto the polymeric matrices compared to the CA control film. The magnetic films (F), containing M1 (Fe 5 C 2 ) and M4 (m-Fe 3 O 4 ) NPs, namely FM1 and FM4 present a more homogeneous surface than the films containing the M2 (Fe 5 C 2 ) and M3 (h-Fe 3 O 4 ) NPs, namely FM2 and FM3 films. Moreover, the structural integrity of all films must be highlighted since there are no observable holes, which is a requirement of quality for films. 3.2.2. Magnetic behavior The magnetic behavior of the magnetic films and respective NPs was studied to understand the interactions and magnetic properties of NPs, providing a better insight into the physics of the magnetic material. VSM analysis was carried out to determine the hysteresis loops and calculate the remanence, the magnetization saturation, and the coercive field. Fig. 4, shows the magnetic properties of both bare NPs and their corresponding magnetic films measured at 26 ◦C. The films consist of Fe 5 C 2 , multicore, and hexagonal Fe 3 O 4 NPs, with concentrations ranging from 0.02 to 0.2 wt%. The magnetic data have been normalized based on the magnetic mass content of each sample. The hysteresis loops in Fig. 4a and b, reveal the ferromagnetic behavior of Fe 5 C 2 NPs (M1 and M2) with a saturation magnetization of Ms=104.3 emu/g Fe3O4 and Ms=109 emu/g Fe3O4 and a coercive field of Hcoer=307.6 Oe and Hcoer=280.4 Oe, respectively (detailed magnetization values in Table S1). The obtained Ms values are slightly higher Fig. 1. TEM images of MNPs (upper images) and size histogram (lower images): (a) Fe 5 C 2 (M1), (b) Fe 5 C 2 (M2), (c) hexagonal Fe 3 O 4 (M3) and (d) multicore Fe 3 O 4 (M4), respectively. L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 5 than reported values, Ms=90 emu/ g (Ahmadpoor et al., 2018) and Ms=95 emu/ g (Z. Yang et al., 2017) for nanoparticles with a diameter size below 100 nm. The hexagonal Fe 3 O 4 (M3) NPs exhibit the characteristics of a soft ferromagnetic material with high saturation magnetization (Ms=90 emu/g Fe3O4 ) and low coercivity (Hcoer=84 Oe) values, as shown in Fig. 4c. Meanwhile, the multicore Fe 3 O 4 (M4) NPs, have a saturation magnetization of 95 emu/g Fe3O4 , which is slightly higher than the reported value for bulk Fe 3 O 4 samples (Ms=92 emu/g) (Kim et al., 2009). This result, may be attributed to the experimental procedure used for determining the magnetic solid content through TGA (Tsioptsias, 2022). Furthermore, the M4 NPs exhibit low coercivity (Hcoer=6.6 Oe) and low remanence (Mrem=9.3 emu/g Fe3O4 ) values, consistent with the behavior of a weak ferromagnetic material. Moreover, the developed magnetic CA films have the same magnetic Fig. 2. FTIR (a) spectra and XRD (b) diffractograms of the MNPs: Fe 5 C 2 (M1), Fe 5 C 2 (M2), hexagonal-Fe 3 O 4 (M3), and multicore-Fe 3 O 4 (M4), the latter with the standard diffraction patterns of Fe 5 C 2 (blue columns) and F 3 O 4 (red columns) NPs. Inset: Zoom-in of the 2900–2850 cm −1 spectral region from M1 and M2 NPs. Fig. 3. SEM images of the films with 0.1 wt% of MNPs; FM1 (Fe 5 C 2 ), FM2 (Fe 5 C 2 ), FM3 (h-Fe 3 O 4 ), FM4 (m-Fe 3 O 4 ) and CA control film without nanoparticles. Zoom inset SEM images included of each film. L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 6 print as the bare NPs at certain NPs concentration. However, there is reduction in the Ms value in magnetic films with 0.02 wt% MNPs content. This behavior is attributed to the diamagnetic contribution of the CA layer, which becomes evident in films with weak magnetization, as observed in Fig. 4e. It is observed that, as the NPs concentration increased, Ms values increased in all samples. For instance, in the FM1 samples with a magnetic content (0.02, and 0.1 wt%), Ms values increased from 90.6 to 97.7 emu/g Fe3O4 , respectively. These results are considerably higher compared to other studies. It was reported in pectinchitosan films containing Fe 3 O 4 NPs, Ms values of 2.38 emu/g (containing 0.1 wt% NPs), and 206.11 emu/g (containing 10 wt% NPs) (Zarandona et al., 2023). Furthermore, in films with cellulose nanocrystals (CNCs) and Fe 3 O 4 NPs with magnetic content of (1, 3, and 5 wt %) the Ms values obtained were (0.4, 0.9, and 1.5 emu/g) respectively (Abdalkarim et al., 2020). The similar magnetic print between the films and NPs enables the design and application of these magnetic films as anti-counterfeiting tags with varying magnetic performance making them suitable for magnetic sensors. Based on their magnetic properties and the uniform distribution of MNPs observed by SEM within the CA matrix, the films FM1 and FM4, both with a magnetic content of 0.1 wt%, were identified as suitable candidates for magnetic tagging and, were therefore thoroughly characterized. 3.2.3. Structural, textural, and topographical properties A detailed assessment of the structure, topography, and textural properties was conducted on the dried magnetic films containing 0.1 wt % of M1 (FM1) and M4 (FM4) NPs. Fig. 5a, shows the FTIR spectra of CA control film and magnetic films with (0.1 wt%) MNPs. In all spectra, a broad absorption peak at 3472 cm −1 is observed, being attributed to the stretching intermolecular hydrogen bonds of hydroxyl groups (-OH). The presence of this peak is attributed to moisture or to non-esterified hydroxyl groups of cellulose (Hwang et al., 2009; Kramar et al., 2023). Furthermore, the FTIR spectra of the CA control film reveal stretching vibration bands at 2945, 1736, and 1028 cm −1 , corresponding to the functional groups -CH, -C – – O, and -C – – OH, respectively. The Fig. 4. Magnetic hysteresis loops of both nanoparticles and magnetic films, including (a) M1, (b) M2, (c) M3, and (d) M4, which have distinct nanoparticle concentrations. The figure also includes (e) the CA control film without NPs. L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 7 vibrational deformation band (-CH 2 ) and the anti-symmetric stretching vibration (-C-O-C-) characteristic of the ester group found in pure CA are located at 1431 and 1220 cm −1 , respectively (Sudiarti et al., 2017). All mentioned bands are also present in the CA magnetic films but with lower intensity and broader shape than the control film due to complexation effect (Ramesh et al., 2012, Selvakumar & Bhat, 2008). Neither Fe-O characteristic in FM4 band nor the characteristic band of Fe 5 C 2 NPs in the FM1 film can be perceived due to the low concentrations of MNPs present in both films. Both samples exhibited similar characteristic features without introducing new peaks. The results demonstrated that only physical bonding occurred between the MNPs and CA. Fig. 5b shows the XRD diffractograms of both the CA control film and the magnetic films. In the diffractogram of the CA control film, is observe two prominent peaks centered at 2Ө=10.2 and 22.8◦, corresponding to the semi-crystalline nature of cellulose acetate. However, these peaks become less pronounced upon the addition of MNPs to form the magnetic CA films. Although XRD analysis suggests that the structural characteristics of cellulose films remain intact when doped with MNPs, the reduction in peak intensity makes it challenging to differentiate the structural presence of MNPs within the films. Notably, there are no distinct reflection peaks corresponding to Fe 3 O 4 or Fe 5 C 2 in the diffractogram. Hence, alternative methods were employed to gain insights into the material’s structure. Confocal Raman spectroscopy was employed to analyze the MNPs distribution, and chemical interactions with CA. Fig. 6, shows the magnetic CA films (FM1 and FM4) both containing 0.1 wt% NPs, and CA Raman spectra. In the spectrum of FM1 film containing the Fe 5 C 2 (M1) NPs, a steep peak at approximately 1272 cm −1 is observed, corresponding to the D band, which is typically found in carbon-based materials. Structural defects on the surface of the as-synthesized Fe 5 C 2 NPs may have occurred, explaining the dominant presence of the Fe 3 O 4 NPs phase observed in the Raman spectrum. Characteristic peaks associated with Fe 3 O 4 NPs located at 391, and 585 cm −1 correspond to the vibration modes of the Fe-O band (C. Huang et al., 2012). These peaks are also detected in the M4 NPs (m-Fe 3 O 4 ), confirming the formation of Fe 3 O 4 NPs. The characteristic fundamental bands of cellulose are present at 1125 and 2940 cm −1 which are attributed to the stretching of C-H and the asymmetric stretching vibration of C-O-C glycosidic linkage, respectively. Additionally, peaks at 1378, 1429, and 1736 cm −1 are linked to asymmetric and symmetric vibrations of (-CH) and of (C – – O) group. The remaining peaks at 656 and 913 cm −1 are associated with (C-OH) bonds (S´ anchez-M´ arquez et al., 2015). Confocal images of the films show the distribution of NPs (red) within the cellulose acetate network (blue). Notably, the dispersion of NPs appears more uniform in FM1 compared to FM4 film. To further assess the surface topography, a 3D optical profilometer was used. Fig. 7 presents both 2D and 3D surface images of the magnetic CA films, covering a scanned area of 0.8 mm 2 . Fig. 5. FTIR spectrum (a) and XRD (b) diffractogram of cellulose acetate films: CA control film, FM1 (0.1 wt% Fe 5 C 2 NPs), and FM4 (0.1 wt% Fe 3 O 4 NPs), respectively. Fig. 6. Confocal Raman spectroscopy of CA, M1 (Fe 5 C 2 ) and M4 (m-Fe 3 O 4 ) NPs, with respective highlighted images of cellulose component (blue color) and NPs M1, and M4 (red color) dispersed in the films FM1, and FM4 with 0.1 wt% NPs. L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 8 Roughness parameters, determined according to ISO 4287:1997, are summarized in Table 1. The total height of the profile (Rt)and root mean squared of the surface roughness (Rq)for the magnetic CA films are significantly higher compared to the control film. FM1 film exhibits a wider and rough surface with Rt=157.01 µm and Rq=39.3 µm in contrast to the FM4 film, which reports values of Rt=1.85 µm and Rq=0.33 µm. The difference between the two films is evident in the 2D and 3D topography images. In the case of FM1 film, the analyzed area reveals more variations in terms of peaks and valleys compared to the FM4 and the CA control film. To quantity specific features of the topography and surface distribution of the films, skewness (Rsk)and kurtosis (Rku) were calculated. Negative values of Rsk <0indicate that all film surface have deeper valleys than peaks, resulting in sharper surface (Rku>3). For FM1 and FM4 films, the values of (Rsk,Rku) are (−0.90, 2.99 µm) and (−0.66, 3.49 µm), respectively. This indicates that FM1 has fewer valleys than FM4, and its surface is less sharply defined. Interestingly, despite SEM revealing a wider distribution of M4 NPs, the roughness parameters suggest that the surface of the FM1 films experiences less disruption, and the Fe 5 C 2 NPs are more uniformly dispersed within the cellulose network compared to the M4 (m-Fe 3 O 4 ) NPs. To further evaluate the surface morphology of the formed films AFM was used. The AFM image of the FM1 (Fig. 8a) shows a uniform distribution of the NPs with visible small aggregates and an average grain size of 10 nm. Meanwhile, the AFM image of the film FM4 contains large particle aggregates and a grain size of 80 nm approximately. These results are in agreement with Fig. 7. Topography images of the magnetic CA films: FM1 (a), FM4 (b) and of the CA control film (c) with respective 3D profile images (right image), respectively. Table 1 Roughness parameters of magnetic CA films. Films Rt* (µm) Rq * (µm) Rku* (µm) Rsk* (µm) FM1 157.1 39.3 2.9 -0.90 FM4 1.9 0.33 3.49 -0.66 CA control 0.35 0.041 3.20 -0.21 *(Rt)is the total height of the profile; (Rq)root mean squared of the surface roughness; (Rku)is kurtosis, and (Rsk)is skewness. L. de Castro Alves et al.
Food Packaging and Shelf Life 42 (2024) 101264 9 the results from the optical profilometer. 3.2.4. Moisture content (MC), solubility, and mechanical properties MC and solubility are important parameters to determine the films’ stability when used as a tag in packaging, where environments with high relative humidity can lead to the modification of films’ properties and thus their performance as a magnetic tag. Table 2 shows the moisture content and solubility of the magnetic (FM1 and FM4 with 0.1 wt% NPs) and of the CA control film. The highest moisture content was seen in the control film. The incorporation of the NPs in the films does not change the films’ main properties of the films, and thus, it can be said that there is a good compatibility between the materials. These results reveal that the incorporation of NPs does not influence the moisture content of the films. Cellulose acetate films are known to have low moisture uptake and solubility compared to other films because of the low OH groups present in their structure, and they are known to be suitable for providing water resistance. Similar behavior was observed in chitosan/cellulose acetate films with CeO 2 NPs for wound dressing (Kalaycıo˘ glu et al., 2020). The mechanical properties of the magnetic CA films, such as tensile strength (TS), elongation at break (EB), and Young’s modulus (YM), were not affected by the presence of the MNPs, as shown in Table 2. The results confirm that the incorporation of MNPs will not impact the mechanical properties of the films. Similar results were observed by Zarandona et al., 2023 for the EB and YM using chitosan-pectin films with low concentrations of iron oxide (Fe 3 O 4 ) magnetic nanoparticles with a size ranging between 50–100 nm. Reported works show that only high concentrations of MNP (e.g. >5 wt%) could significantly affect the mechanical properties of biopolymer-based films (Mehmood et al., 2020; Zarandona et al., 2023). It is important to highlight that these results are in accordance with reported studies taking into account the mechanical properties of biopolymer films, where tensile strength values between 0.002 to 46.5 MPa and low-density polyethylene (LDPE) values between 9–17 MPa were reported (Galus et al., 2020). Generally, biopolymers have lower EB values than conventional plastics (Silva et al., 2020), but these properties will guarantee their use as a tag in a packaging material. 3.2.5. Opacity and color Opacity is an important parameter used to measure the light intensity passing through a material controlling the incidence of light on packaged food offering a barrier against oxidative processes. Fig. 9 shows digital photos of the CA control and magnetic films. The films with NPs (FM1 and FM4) are darker in color than the CA control film, and no additional difference is observed. Table 3 presents the opacity and color parameters values of the films. The results indicate higher opacity values in magnetic films. Additionally, the a* values of the magnetic CA films suggest a more reddish color and yellower appearance (b*) than the CA control film. Conversely, the addition of 0.1 w.% of M1 and M4 NPs led to a decrease in the lightness Fig. 8. 2D AFM surface topography images for: FM1 (a), FM4 (b) and CA control film (c) with respective 3D image (below). Table 2 Values of moisture content and water solubility, tensile strength (TS), elongation-at-break (EB) and Young’s modulus (YM) of the magnetic CA and control films. Films Moisture content (%) Solubility (%) TS (MPa) EB (%) YM (GPa) FM1 6.6 ±0.9 a 2.2 ±0.3 a 52.3 ±7.1 a 3.5 ±0.9 a 24.8 ±1.79 a FM4 6.9 ±0.5 a 2.6 ±0.3 a 51.9 ±5.8 a 2.9 ±0.3 a 24.5 ±3.7 a CA control 7.1 ±0.3 a 2.5 ±2.0 a 55.5 ±4.5 a 3.8 ±0.6 a 23.2 ±5.7 a Values reported are the means ±standard deviations. Different letters a–b in the same column indicates a statistically significant difference among different samples (p<0.01). L. de Castro Alves et al.