scieee AI-readable full text Open interactive document viewer

Theoretical and computational study of thermal and electric transport processes in nanostructured systems

Carrete Montaña, Jesús

Abstract

This thesis concerns itself with the theoretical and computational study of the thermal and electric conduction properties of two kinds of nanostructured systems: semiconductor nanostructures and ionic liquids. In particular, chapters are devoted to the thermal conductivity of InP, InAs and GaAs nanowires, calculated through molecular dynamic methods, to the study of the thermal conductivity of Si nanowires with rough surfaces using Green's functions, to the thermoelectric properties of hybrid organic-inorganic superlattices, to the electric and thermal conductivities of ionic liquids and their mixtures with a solvent, and to the nanostructure of such mixtures. Results are compared to experimental data whenever possible.

Full text

Tesis doctoral THEORETICAL AND COMPUTATIONAL STUDY OF THERMAL AND ELECTRIC TRANSPORT PROCESSES IN NANOSTRUCTURED SYSTEMS Jesús Carrete Montaña D. Luis Javier Gallego del Hoyo, Catedrático del Departamento de Física de la Materia Condensada, y D. Luis Miguel Varela Cabo, Profesor Titular del mismo Departamento, de la Universidad de Santiago de Compostela INFORMAN: Que el trabajo titulado Theoretical and computational study of thermal and electric transport processes in nanostructured systems ha sido realizado bajo su dirección por D. Jesús Carrete Montaña en el Departamento de Física de la Materia Condensada de la Universidad de Santiago de Compostela, y constituye la memoria para optar al grado de Doctor en Física. Santiago de Compostela, 30 de abril de 2012. Prof. Luis Javier Gallego del Hoyo Prof. Luis Miguel Varela Cabo Summary In the present thesis a theoretical and computational study of transport phenomena is performed for two kinds of nanostructured physical systems of very different characteristics but sharing the common feature of technological interest: semiconducting nanostructures and ionic liquids. Following this plan, it is structured in two parts, each one dealing with one of these classes of systems, even though there is a relation of thematic unity and methodological overlap between both of them. Placed before these thematic blocks, a brief chapter tries to explain the reasons for this choice of topic, as well as the global aims of this work. Part I of this document is devoted to nanostructured semiconductor materials. The need for further miniaturisation in modern electronics together with the desire to explore the exciting possibilities offered by the nanoscale call both for methodological innovations in this field and for the generation of results with regard to promising nanostructures. Of course, given the almost infinite variety of structures which can be built from atoms of semiconductor materials, some particular instances had to be chosen. Thus, Chapter 2 addresses the thermal conductivity of indium phosphide nanowires through direct non-equilibrium molecular dynamics methods. First, some concepts about thermal conduction in the nanoscale are introduced; next, the methodological choices made for this chapter are explained and justified. Finally, numerical results for the thermal conductivity of such quasi-one-dimensional nanostructures are presented and compared with those obtained by other authors for Si nanowires. Apart from the fact that the order of magnitude of the results is certainly beneath that of bulk InP, the main conclusion is that a small enhancement in thermal conductivity happens when the diameter of the wires is reduced below a certain point. An explanation for this phenomenon is given in terms of an approximate phonon density of states, also obtained by molecular dynamics. One of the main choices in any molecular dynamics simulation is the interaction potential, which must be judged in terms of its transferability to the situation under study. Chapter 3 contains thermal conductivity calculations v for InP, InAs and GaAs nanowires done employing the same methods as in Chapter 2 but using, in each case, two very different potentials: on one hand, the Branício-Rino potential for InP and the similarly complex Hammerschmidt potential for arsenides, in whose parameterisations their authors have taken vibrational properties into account; on the other, the Harrison potential, a very simple, biparametric and quasi-harmonic model shown by previous authors, by semi-analytic methods, to yield results an order of magnitude below those in Chapter 2. The molecular dynamics results presented in this chapter show that the Harrison potential can afford correct predictions of the qualitative trend of thermal conductivity as a function of nanowire diameter, but generally results in concrete values well below those obtained using the more sophisticated interaction potentials. In order to gain further insight into this phenomenon, the elements of the harmonic description of vibrations in solids are introduced in this chapter and the phonon densities of states associated to each potential are calculated in this formalism. The Harrison potential is shown as unable to reproduce these densities with a level of detail comparable to the other options tried. Thus, a correct choice of the interaction potential, bothregarding its functional form—whichmustbeadjustedtotheunderlying physics — and its parameterisation — which must include magnitudes related to thermal conductivity — is essential in molecular dynamics simulations of heat transfer in nanostructures. Due to the limitations of molecular dynamics methods, starting with Chapter 4 thermal conduction is treated from the beginning as a phonon transmission problem. The systems chosen in this case are nanowires made from Si, the central element in electronics. For sufficiently thin nanowires, phonon scattering should be dominated by the nanowire boundary. In more macroscopic wires with rough boundaries that cause isotropic reflection of phonons, its influence translates into a phonon mean free path proportional to the diameter of the system. However, some experimental results point to values of the thermal conductivity well below those which could be expected if this result (known as Casimir’s formula) held for thin wires. A theoretical study also managed to explain these experimental measurements, but seemingly did so at the expense of methodological correctness, as it made use of Fermi’s golden rule outside its aprioristic domain of applicability and included boundary effects twice. In order to check the validity of Casimir’s formula for very small diameters and to determine if the aforementioned experimental data can be explained exclusively in terms of boundary scatvi tering, a purely atomistic study was performed. Chapter 4 introduces the main elements behind this piece of research — the Stillinger-Weber potential, the non-equilibrium Green’s function formalism and a simple form of the Boltzmann transport equation — and how they were combined in order to obtain the conductivities of thin silicon nanowires with a rough boundary. Using these tools, two scenarios were considered, shallow and deep surface disorder. The results show that Casimir’s mean free path is a good approximation for shallow roughness (like that presumably present in the experimental situation) even for diameters as small as 2.22nmbut that a thermal conductivity significantly below this limit can be achieved using very deep defects, even though they might compromise other desirable properties. Therefore, a disordered boundary is not enough to explain the very low conductivities detected experimentally, and the theoretical success previously mentioned seems attributable to methodological errors. In addition to this, Chapter 4 contains some novel theoretical work and formulas that allow detailed phonon transmission probabilities across a localised defect to be calculated from knowledge of the causal 𝑡-matrix of the defect. Chapter 5 closes the first part of this work with a study about a new kind of material: hybrid organic-inorganic superlattices built from alternated layers of aSiGealloy and self-assembled monolayersoforganicmolecules(tri-tiophene, in this particular case). Research about such systems is in its infancy, but they seem to hold great promise for thermoelectric applications, i.e., for the movement of heat against a thermal gradient through the use of electric power or for the generation of electricity by harnessing temperature differences. In order to have a thermoelectric material able to compete with more traditional energy conversion cycles it is necessary to achieve a high ratio between its electric and thermal conductivities, which has been so far impossible using semiconductors alone. The soft molecular interfaces in hybrid superlattices, however, could be able to scatter phonons very efficiently while maintaining a reasonable electric conductivity due to the conjugate orbitals present in the particular organic molecules chosen. In order to study such a complex system, methods from Chapter 4 are again applied to phonon transport and a similar formalism — based on the Boltzmann transport equation in the relaxation time approximation — is introduced for electrons, after briefly discussing the phenomenological description of thermoelectric conversion. A combination of ab-initio calculations and semiempirical interaction models is used as the input. The results obtained are promising, since even though the organic layers impede vii electron transport to a certain degree, they block phonons much more dramatically, resulting in extremely low thermal conductivities, in the order of magnitude of 0.1W/(mK). Therefore, the dimensionless thermoelectric figure of merit (a combination of factors which determines the efficiency of a thermoelectricmaterial)ofthe studiedsuperlatticesislargerthanthat of SiGe alone by a factor of more than two, regardless of whether ballistic or ohmic transport is assumed. Moreover, the simple addition of a phenyl group to each of the oligothiophenes in the organic layers causes a variation of more than 20%in the results, suggesting that the thermoelectric properties of these hybrid heterostructures can be tuned (and therefore optimised) using organic chemistry techniques to exploit the almost infinite flexibility of carbon-based molecules. Part II of this thesis is devoted to the study of ionic liquids, a label applied to those substances with melting points below 100∘Cthat are completely dissociated into ions. Their versatility as solvents and the relative ease with which they may be separated from the products of a reaction without losses to the environment makes ionic liquids one of the cornerstones of “green chemistry”. Theirtransportpropertieshavebeen studiedalmostfromthe very discovery of this kind of substance, and remain extremely important today as ionic liquids are being considered as reaction media (which must also act as thermostatic baths) and for electrochemical applications. The study of liquid-state systems is notably complex, in part due to the absence of an ideal reference system, and very rarely can the level of predictive power often seen in solid-state theories be achieved. Instead, the results of theoretical investigations about liquids are often semi-quantitative models capable of explaining particular trends, sometimes with the help of parameters obtained from experiment. Nonetheless, even for liquids a good model must go beyond being an useful metaphor: it must be based on experimental observations and show some transferability to the study of different variables. For ionic liquids, a particularly interesting frameworkwhenjudgedinthelightthesecriteriaistheBahe-Varelapseudolat- tice theory. Its underlying hypothesis, backed by results from X-ray scattering experiments, is the existence of a statistically regular arrangement of atoms in ionic liquids and their mixtures, as well as in concentrated solutions of conventional electrolytes. This theory has been successfully used to predict various equilibrium properties of these kinds of liquid systems. It is a relatively well-known fact, indirectly inferred from experimental and simulation studies, that the nanostructure of ionic liquids and their mixtures with a solvent plays a crucial role in determining their properties. viii However, very few works in the literature address this problem directly. Chapter 6 does so from two different points of view, as a prelude to the remainder of Part II. First, ionic and solvent cluster formation inside mixtures of 1-buthyl-3-methylimidazolium with water, methanol and ethanol is studied, reaching the conclusion that while water has a marked tendency to form big clusters — inside which water molecules experience a bulk-like environment — alcohols are only found in clusters of rather modest sizes, even at very high concentrations. Moreover, ions form a polar network that is not broken until there is a lot of solvent present in the mixture. Such breakdown occurs abruptly when the solvent is water, but passes through an intermediate regime with big ionic clusters present when the solvent is an alcohol. The second method used to study the microscopic structure of these mixtures is based on diagrams showing the conditional probability that a solvent molecule at a particular distance from a central ion has a given orientation, i.e., diagrams of the angular structure of solvation layers. In those, the differences between water and alcohols can also be clearly appreciated. In Chapter 7 a theoretical model is developed, based on the Bahe-Varela formalism, for the electric conductivity of conventional electrolyte solutions, ionic liquids and their mixtures with solvents. The central concept in this theoretical proposal is that of a cooperative rearrangement region, and electric conduction processes are explained in terms of random hops between these regions, whose probabilities are affected by the application of an electric field. Ion-ion and ion-solvent interactions are explicitly included by combining a path probability method with a Bragg-Williams-like approximation for interparticle interactions. A simple hypothesis of uncorrelated ion motion leads to the prediction that electric conductivity as a function of the volume fraction of ionic liquid has a maximum due to competition between two opposite effects, an increase in the density of charge carriers and a decrease in their mobility. When the conductivity curve is expressed in a reduced form, by dividing both the conductivity itself andthe volume fractionbytheirvaluesatthemaximum, the theoretical model predicts an universal behaviour, i.e., a correspondingstates law. Comparison with experiment shows excellent agreement between this theoretical results and the real behaviour of the systems under study. Deviations from the corresponding-states law depend on the solvent and can be qualitatively explained in terms of cluster formation, using results from Chapter 6. Finally, the thermal conductivity of ionic liquids and their mixtures is studix miempíricas. Los resultados obtenidos resultan prometedores, pues aunque las monocapas orgánicas bloquean el paso de electrones en cierta medida, dificultan mucho más la conducción de fonones. De este modo, pese a que se observa una reducción de las magnitudes que describen el transporte eléctrico con respecto a la aleación SiGe en forma de sólido masivo, la espectacular reducción de la conductividad térmica — cuyo valor para la superred puede caer hasta el orden de magnitud de 0,1W/(mK)— hace que la cifra de mérito termoeléctrica mejore a la del SiGe aislado en un factor ∼2,5, tanto si se supone que el transporte es óhmico como si se usan períodos de la superred lo suficientemente cortos para suponer que el transporte térmico es balístico. Más aún, la simple adición de un grupo fenil a cada uno de los politiofenos que forman las monocapas provoca una variación del 20%en los resultados, lo que indica que las propiedades termoeléctricas de este tipo de materiales nanoestructurados son susceptibles de ser modificadas, y en consecuencia optimizadas, utilizando toda la potencia de los métodos de la química orgánica para aprovechar la infinita flexibilidad de las moléculas basadas en el carbono. La Parte II de la tesis aborda el estudio de un tipo diferente de sistemas nanoestructurados, los líquidos iónicos. Se clasifican bajo esta denominación aquellas sustancias cuya temperatura de fusión se encuentra por debajo de los 100∘Cy que están compuestas completamente por iones, esto es, disociadas por completo. Los líquidos iónicos cuentan ya con unos cien años de historia y componen una numerosísima familia cuyas particulares propiedades — presión de vapor prácticamente nula, amplio rango de temperaturas de trabajo, etc. — y su versatilidad como disolventes les proporcionan un gran interés industrial, como alternativa a disolventes más convencionales y como piezas clave de la llamada “química verde”, en la cual se intentan minimizar los residuos generados. Las propiedades de transporte de los líquidos iónicos han sido estudiadas desde el mismo instante de su descubrimiento y revisten hoy gran importancia. Así, la conductividad térmica de estos sistemas es crucial de cara a su utilización como medios de reacción — ya que una de sus funciones en ese papel será servir como baño termostático para el proceso químico —, como lubricantes, como fluidos caloportadores o como refrigerantes. Por otro lado, su conductividad eléctrica es uno de los parámetros de interés para la aplicación de estos líquidos a procesos electroquímicos (p. ej., como disolventes en electrolitos de baterías). Tales magnitudes son objeto de estudio en esta parte del trabajo, que busca establecer teorías de aplicabilidad suficientemente general. Debe tenerse presente que el estudio de sistemas en estado xvi líquido es notablemente complejo debido, entre otros factores, a la falta de un sistema de referencia ideal, y que por consiguiente rara vez se puede llegar a resultados que exhiban el mismo poder predictivo que teorías similares de estado sólido. En lugar de esto, a menudo el resultado de las investigaciones teóricas son modelos semicuantitativos capaces de explicar determinadas tendencias, quizás con ayuda de parámetros obtenidos de los experimentos. Sin embargo, también en estado líquido un buen modelo debe sustentar sus hipótesis en observaciones reales. Otro criterio importante para juzgar la calidad de estos desarrollos es su transferibilidad al estudio de diferentes variables. En el estudio de líquidos iónicos, un marco teórico que cumple muy bien estos dos requisitos es el formalismo pseudorreticular de Bahe-Varela. Su hipótesis subyacente, respaldada por estudios de rayos X, es la existencia de un arreglo reticular estadístico en el seno de estos líquidos, y ha sido usado para predecir diversas propiedades de equilibrio y transporte. En consecuencia, fue este el formalismo elegido para esta parte de la tesis. Es un hecho relativamente bien conocido, o cuando menos inferido indirectamente a partir de resultados experimentales y de simulación, que la nanoestructura de los líquidos iónicos y sus mezclas con disolventes es crucial para entender sus propiedades. Son pocos en la literatura, sin embargo, los estudios que se ocupan del tema directamente. El Capítulo 6 lo hace desde dos puntos de vista, a modo de preludio al resto de la Parte II. En primer lugar, se estudia la formación de agregados de iones o de moléculas de disolvente en mezclas de tetrafluoroborato de 1-butil-3-metilimidazolio con agua, metanol y etanol. De este estudio se extrae la conclusión de que, mientras el agua tiene una gran tendencia a formar grandes agregados dentro de los cuales sus moléculas experimentan un entorno semejante al del agua pura, los alcoholes no lo hacen ni siquiera a concentraciones muy altas. Por su parte, los iones tienden a formar una red polar dentro de la mezcla que no se rompe hasta que se ha añadido mucho disolvente. Dicha ruptura es relativamente abrupta cuando el disolvente es agua, pero en el caso de los alcoholes pasa por un estadio intermedio en el que están presentes grandes agregados de iones. El segundo método de estudio de la estructura microscópica de estas mezclas son los diagramas de probabilidad de que las moléculas de disolvente adopten una orientación determinada a cada distancia de un ion central, es decir, diagramas de la estructura angular de las diversas capas de solvatación. También aquí surgen contrastes entre el agua y los alcoholes, que se relacionan con la formación de agregados. xvii En el Capítulo 7 se desarrolla un modelo teórico, basado en el citado formalismo pseudorreticular, para la conductividad eléctrica en líquidos iónicos y sus mezclas con disolventes, así como para disoluciones electrolíticas convencionales. El concepto central en esta propuesta teórica es el de región de reorganización cooperativa, y los procesos de conducción eléctrica se explican en términos de saltos aleatorios entre estas regiones, cuyas probabilidades se ven afectadas por la presencia de un campo eléctrico. Las interacciones ion-ion e ion-disolvente se incluyen de manera explícita combinando un método de probabilidad de camino obtenido de la bibliografía con una aproximación de tipo Bragg-Williams para las interacciones entre partículas. Admitiendo movimiento iónico no correlacionado se llega a la predicción de que la conductividad eléctrica, tratada como función de la fracción volúmica de disolvente, posee un máximo que surge de la competición entre el aumento de la concentración de portadores de carga y la disminución de su movilidad. Cuando esta curva de conductividad se expresa en términos de magnitudes reducidas, la teoría predice un comportamiento universal. La comparación con resultados experimentales para líquidos iónicos y sus mezclas y para disoluciones salinas arroja un acuerdo excelente en lo tocante a esta ley de estados correspondientes. Las desviaciones con respecto al comportamiento universal se explican, cualitativamente, recurriendo a resultados sobre formación de agregados obtenidos en el Capítulo 6. La conductividad térmica de líquidos iónicos y sus mezclas es el tema central del Capítulo 8. Partiendo de nuevo de la teoría de Bahe-Varela, se recuperan y adaptan conceptos de la teoría de transporte en sólidos cristalinos ya usados extensivamente en la Parte I. Con base en la literatura, se precisa el sentido del concepto de modo normal en un líquido y se analizan estos modos y su extensión espacial para dos líquidos iónicos puros. A continuación se plantea una imagen del líquido iónico correspondiente a la existencia de orden de medio alcance: regiones ordenadas separadas por barreras efectivas. Esta imagen se asemeja a la situación existente en otros sistemas físicos como los sólidos policristalinos y amorfos. Este tipo de estructuras presentan el grado suficiente de orden (en forma de simetría de traslación aproximada en un entorno local) para permitir la existencia de modos vibracionales comparables a fonones. Aquellos de entre estos modos que tengan una longitud de onda mayor que la anchura característica de una barrera podrán propagarse y transmitir calor, mientras que los de longitud de onda pequeña tenderán a estar confinados en un dominio ordenado. Tal mecanismo de transferencia de xviii calor se conoce como phonon hopping. En este capítulo se desarrolla un modelo de conducción térmica basado en el mismo y, mediante algunas hipótesis adicionales que permiten un tratamiento analítico, se llega a resultados cualitativos para líquidos iónicos puros, así como a una fórmula de interpolación sin parámetros para sus mezclas con disolventes. La comparación con datos experimentales para mezclas de líquidos iónicos basados en el anillo imidazolio con agua y etanol pone de relieve la gran importancia de la nanoestructura del líquido: mientras que en mezclas con agua un tratamiento del disolvente basado en sus propiedades como sistema masivo arroja un excelente acuerdo con la experiencia, para alcoholes es claramente necesario un estudio más sofisticado como función de la concentración. Se interpreta este hecho como reflejo de la rápida aparición de agregados de agua en el seno de la mezcla y de su ausencia en el caso del alcohol. Se cierra esta tesis con un breve capítulo en el que se resumen, de manera esquemática, las principales conclusiones. xix Agradecimientos Es frecuente escuchar que, mirando hacia atrás, el tiempo vivido siempre parece corto. Tras mi paso por la Facultad de Física, no podría estar más en desacuerdo: subjetivamente, aquel día de septiembre de 2002 en que entré en ella queda siglos atrás,y se me antoja que este documento acaso no recoja cinco años, sino toda una vida, de trabajo. Por ello, no son pocas las personas a las que en justicia debo mencionar aquí por haberme facilitado el llegar hasta este punto: ▶Mis directores, que no sólo me han transmitido el “mester de investigación” sino un apoyo constante en lo científico y en lo humano. ▶El Dr. Natalio Mingo, mi supervisor en el CEA de Grenoble y gran experto en el transporte térmico, por haberme aceptado bajo su tutela y por la desinteresada atención y la ayuda prestadas durante mis meses de estancia. ▶Mis compañeros del Grupo de Nanomateriales y Materia Blanda, entre los que no puedo pasar sin señalar a Verónica Fuentes, mi primera compañera de despacho, a Roberto Longo, amigo y maestro en todo lo relativo a la DFT, y a Trinidad Méndez, junto a quien he tenido la oportunidad de echar a andar el trabajo de simulación de líquidos iónicos. ▶El profesor Óscar Cabeza y su grupo experimental de la Universidade da Coruña, que me han permitido usar sus datos sobre líquidos iónicos. ▶Los profesores J. Ferrer (Universidad de Oviedo), J. P. K. Doye (Universidad de Oxford) y R. M. Lynden-Bell (Universidad de Cambridge), con quienes he aprendido mucho durante visitas de investigación más breves. ▶Todos aquellos, aparte de los ya citados, que han firmado conmigo alguna publicación, contribuyendo con sus conocimientos a mi evolución científica. xxi ▶Los equipos de desarrollo de SIESTA y GROMACS, por poner a disposición de la comunidad de investigadores estos potentes conjuntos de herramientas sin coste alguno, así como los responsables de la creación de Python y su ecosistema de bibliotecas científicas, empleadas exhaustivamente en todas las etapas del proceso que ha llevado a esta tesis. ▶El personal de la USC, especialmente Minia García y Benito Doce, por su eficaz gestión, y “sir” Jan Coleman, por su asesoramiento lingüístico y su puesta en valor de la palabra artifactually. ▶Mis amigos en España y en Francia, y entre ellos aquellos sin los cuales no hubiese podido viajar: Xesús Bendaña, Lucía González Gato y Zhao Wang. ▶Ana, fuente inagotable de momentos felices, mi familia, a quienes debo todas las oportunidades que he tenido en mi vida, y también mi familia política, que ha supuesto para mí un gran apoyo en Santiago. Tambiéndeseoagradeceral CentrodeSupercomputacióndeGalicia lasnumerosas horas de procesador puestas a mi disposición. Por imperativo legal, también agradezco a las distintas encarnaciones del Ministerio de Educación su financiación de mi trabajo mediante una siempre menguante beca del programa de Formación de Profesorado Universitario (FPU). xxii Contents 1 Motivation and purpose 1 References .................................. 4 I Semiconductor nanostructures 7 2 MD predictions of the thermal conductivity of thin InP nanowires 9 2.1. Introduction.............................. 9 2.2. Intermolecular potential . . . . . . . . . . . . . . . . . . . . . . . 15 2.3. Integrationmethod.......................... 18 2.4. Calculation of the thermal conductivity . . . . . . . . . . . . . . 20 2.5. Characterisation of the phonon densities of states . . . . . . . . 25 2.6. Computational details . . . . . . . . . . . . . . . . . . . . . . . . 26 2.7. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 27 References .................................. 36 3 Influence of the potential on MD thermal conductivity 41 3.1. Introduction.............................. 41 3.2. Details of the MD simulations and of the model potentials . . . 43 3.3. Calculation of the phonon density of states . . . . . . . . . . . . 45 3.4. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 49 xxiii Contents References .................................. 53 4 Surface roughness and thermal conductivity of Si nanowires 57 4.1. Introduction.............................. 57 4.2. Quasi-ballistic transport . . . . . . . . . . . . . . . . . . . . . . . 59 4.3. Transmission calculations . . . . . . . . . . . . . . . . . . . . . . 61 4.4. Infinite rough nanowires: the ohmic regime . . . . . . . . . . . . 68 4.5. The Casimir mean free path . . . . . . . . . . . . . . . . . . . . . 70 4.6. The Stillinger-Weber potential . . . . . . . . . . . . . . . . . . . . 71 4.7. Computational details . . . . . . . . . . . . . . . . . . . . . . . . 72 4.8. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 74 References .................................. 81 5 Thermoelectric properties of hybrid organic-inorganic superlattices 83 5.1. Introduction.............................. 83 5.2. Thermoelectric coefficients . . . . . . . . . . . . . . . . . . . . . . 87 5.3. Transmission calculations . . . . . . . . . . . . . . . . . . . . . . 91 5.4. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 98 References ..................................104 II Ionic liquids 107 6 Nanostructure of imidazolium-based ionic liquids 109 6.1. Introduction..............................109 6.2. Simulationdetails...........................114 6.3. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 117 References ..................................135 7 Pseudolattice theory of electric conductivity 139 7.1. Introduction..............................139 7.2. Experimental details . . . . . . . . . . . . . . . . . . . . . . . . . 143 7.3. Theoretical section . . . . . . . . . . . . . . . . . . . . . . . . . . 143 7.4. Results and discussion . . . . . . . . . . . . . . . . . . . . . . . . 148 References ..................................155 8 Heat transport in a pseudolattice 159 8.1. Introduction..............................159 8.2. Vibrational spectrum of an IL . . . . . . . . . . . . . . . . . . . . 162 xxiv Contents 8.3. Thermal conduction mechanism . . . . . . . . . . . . . . . . . . 168 8.4. Experimental procedure . . . . . . . . . . . . . . . . . . . . . . . 172 8.5. Discussion for pure ILs . . . . . . . . . . . . . . . . . . . . . . . . 173 8.6. Mixtures with a solvent . . . . . . . . . . . . . . . . . . . . . . . . 174 References ..................................178 9 Conclusions 181 List of Tables 185 List of Figures 187 List of publications related to this thesis 193 Complete references 197 xxv Part I Semiconductor nanostructures 7 2Molecular dynamics predictions of the thermal conductivity of thin InP nanowires So many of the properties of matter, especially when in the gaseous form, can be deduced from the hypothesis that their minute partsareinrapidmotion, the velocity increasing with the temperature, that the precise nature of this motion becomes a subject of rational curiosity. Illustrations of the Dynamical Theory of Gases James Clerk Maxwell 2.1. Introduction Nanowires are quasi-one-dimensional structures whose transverse cross section seldom exceeds the thousands of square nanometers, but which can reach the centimeters in length [19]. Although some organic structures suit these requirements, and inorganic nanowires have also been found in nature, it has been only in the last few decades that the ability to create synthetic nanowires has become widespread. Accordingly, in recent years these nanostructures have attracted considerable research effort for both theoretical reasons — the desire to understand how electronic, optical, thermal and mech- 9 2. MD predictions of the thermal conductivity of thin InP nanowires anical properties are affected by the reduction of dimensionality — and with a view to their potential technological applications of (see, e.g., Refs. 20–22). Nanowires are obvious candidates for the development of miniaturised versions of devices which, in their non-nanoscale versions, show a similarly large aspect ratio. Examples of this are optical fibres and electronic interconnects. However, nanowires also show unique properties absent from their bulk counterparts, caused by the incomparably greater relevance of quantum confinement and surface effects. One of them is their notable tensile strength [23], whichhas stimulatedresearch in nanowires as possible additives forstructural materials. Transport properties form another important group of attributes of these quasi-one-dimensional structures which can be expected to differ from their values in the bulk. Currently, scientific and engineering work is well underway to deliver viable nanoelectronic devices, and already two years ago there were direct methods for creating relatively complex and functional silicon-nanowire- based electronic building blocks, such as logic gates [24]. In this context, information on the thermal conductivity of semiconductor nanowires is crucial for the development of new nanoelectronic and thermoelectric devices. Extremely high thermal conductivity is essential if nanowires are to be used as heat sinks in future nanochips [25, 26], and ultralow thermal conductivity, below 1W/(Km), in conjunction with high electric conductivity and large Seebeck coefficients, if they are to form the basis of efficient thermoelectric refrigerators and power generators [11, 27–29]. Only for a few relatively thick nanowires has thermal conductivity been determined experimentally [30–35]; and because of their relevance tothe semiconductor industry, much of this work has been concerned with Si nanowires [30, 34, 35]. Over the temperature range 20−320K, the thermal conductivities of Si nanowires with diameters of 22,37,56and 115nmhave been reported to be about two orders of magnitude smaller than those of bulk Si and to decrease with decreasing nanowire diameter, a trend that is attributed to the concomitant increase in surface/volume ratio, which enhances the scattering of long-wavelength phonons (the dominant heat carriers) by the nanowire boundary [30]. Such possibility will be studied in detail in Chapter 4. The results of theoretical studies [36–38] and computer simulations [39–41] are in qualitative agreement with these experimental findings. For example, in the temperature range 200−500Kclassical molecular dynamics (MD) simulations of Si nanowires with square cross sections of side 1.61−5.35nm, performed 10 2.1. Introduction by Volz and Chen [39] using the Green-Kubo method [42] in conjunction with the Stillinger-Weber (SW) model of Si-Si interactions [43, 44], found thermal conductivities of 1−5W/(mK)(one to two orders of magnitude smaller than the corresponding bulk value) that decreased with nanowire diameter. Interestingly, however, MD simulations using the “direct” method [42] with the SW potential show that for tetrahedral Si nanowires oriented along the [111]direction thermal conductivity decreases as wire diameter is reduced from 7.7to 3.4nm, but then increases as diameter is further reduced to 1.46nm; this is attributed to a more subtle phonon confinement effect manifested in the fact that the excited mode of lowest frequency and longest wavelength shifts to higher frequency [41]. The thermal conductivities of Si34- and Si46-clathrate nanowires increase with decreasing diameter over the whole range investigated (2−8nm), although only very slightly [41]; the similar but more pronounced diameter dependence of the room-temperature specific heat of thin Si [111]nanowires that is predicted by lattice dynamics theory and MD/SW simulations [45] has likewise been attributed to the combination of phonon confinement and the increase in specific free surface area [45]. In the light of the above results, Si-based nanowires seem unlikely to be very suitable for the applications mentioned earlier, although roomtemperature thermal conductivities of 0.75W/(mK)have been achieved with heavily doped Si [46]. An alternative nanowire material that has attracted considerable attention is InP. InP nanowires have been synthesised by several methods [47–52], and their energy band gaps and photoluminescence images and spectra have been determined experimentally [53, 54]. Furthermore, 𝑝−type doped InP nanowires function as light-emitting diodes and field effect transistors when assembled with 𝑛−type nanowires [55, 56], and the impurity state responsible for current flow in Zn-doped InP nanowires has been characterised [57] by first-principles calculations using PARSEC [58, 59], a real-space implementation of density functional theory and pseudopotentials. However, apparently hitherto there have been no systematic experimental or computational studies of the thermal conductivity of InP nanowires, although theoretical calculations using phonon dispersion relations based on the somewhat crude Harrison potential [60] have been performed for wires 35−10000nmthick at 300Kby Mingo and Broido [61] and Mingo [62]. In the work described in this chapter the thermal conductivity of hexagonal InP nanowires was investigated by means of classical MD simulations using a potential proposed by Branício and Rino [63] that, like the SW potential for Si 11 2. MD predictions of the thermal conductivity of thin InP nanowires [43] and the potentials developed by Vashishta and coworkers for other semiconductor materials [64–67], comprises both two-body and three-body terms. This potential has proved to be very useful for interpreting the vibrational properties and structural phase transformations of bulk InP under pressure [63, 68], but this is the first time that it has been applied to nanowires. Given the lack of systematic experimental studies of the thermal conductivity of InP nanowires, the references taken for comparison were Mingo’s theoretical results [61, 62], and experimental [30, 35], theoretical [36–38] and computational [39–41] results for thin Si nanowires. The thermal conductivity 𝜅of a material is defined as the phenomenological coefficient which links the heat current𝑗𝑄to the temperature gradient ∇𝑇 under a particular set of constraints. In other words, for a particular choice of thermodynamic forces that includes ∇𝑇,𝜅is defined by the relation 𝑗𝑄=−𝜅∇𝑇, (2.1) known as Fourier’s law, when every other thermodynamic force is zero. Depending on the symmetry properties of the material, 𝜅can be an order-2tensor or even depend on the position. It must be noted here that throughout this work the expression “heat current” will be used to denote an energy transfer per unit time and unit area, as opposed to “heat flux”, its integral over a finite surface, even though the opposite convention can also be found in the literature. The application of this terse formula to nanoscale problems is fraught with conceptual difficulties, of which at least three main sources can be identified: What is heat? In most modern formulations of thermodynamics heat it not a central concept but rather a historical burden, as the principles on which this theory is based are introduced without making reference to it. In particular, the concept of entropy, concomitant with the notion of irreversibility, arises in the context of the second law as a consequence of the order induced by the relation of adiabatic accessibility. Under adiabatic constraints, the first law establishes that the work done by a system is equal to the variation of the internal energy, in analogy with the behaviour of a purely mechanical system. Under non-adiabatic conditions, heat is simply the term that is necessary to introduce in the equation of balance to fulfil the conservation of energy. In fact, in the wellknown framework proposed by Lieb and Yngvason [69] as the culmina- 12 2.1. Introduction tion of the approach to the second law pioneered by Carathéodory [70] and largely developed by Buchdahl [71], Boyling [72] and others, heat is neither used nor even defined. Experimentally, there is no way to measure heat directly; instead, an energy transfer is inferred by its effects, and then classified as heat by virtue of the constraints put in place for the experiment. Unfortunately, constraints that arise very naturally in macroscopic hydrostatic systems (constant volume, for instance) have a more nebulous interpretation in the nanoscale. Can a meaningful ∇𝑇be defined? Clearly, temperature cannot be considered from a purely mechanical point of view. The non-mechanical quantity from which it is derived, entropy, is well-defined for equilibrium and non-equilibrium, large and small, hamiltonian and non-hamiltonian, and physical and non-physical systems alike, as long as they can be assigned a set of possible states, but only from a global perspective. The view that it can be used as a local potential from which to derive thermodynamic forces has been described as purely metaphoric [73] and depends on an approximate decoupling between state variables for different volume elements. Can the linear regime be expected to hold? As mentioned above, Fourier’s law is purely phenomenological in nature, and a priori expected to be most useful when |∇𝑇|is suitably small. However, a drop of a few kelvin over a length of 100nmleads to a temperature gradient in the order of 10􀁴K/m, enormous by macroscopic standards. The in-depth exploration of these problems falls outside the scope of this thesis, so they will only be treated insofar as decisions had to be made in order to resolve the ambiguities that they introduce. However, it is important to stressthatthetheoreticalfoundationsof non-equilibrium thermodynamics are still an area of active research, and that simulation results can only be fully justified a posteriori, by comparison with experiment. In practice, heat is defined as the transfer of energy not due to a change in the deformation coordinates of the participating systems (parameters of their hamiltonians in quantum descriptions) and a hypothesis of local equilibrium is introduced in order to be able to define a local temperature. How these hypotheses are implemented depends on the set of techniques available. 13 2. MD predictions of the thermal conductivity of thin InP nanowires At room temperature, nanowires resemble a crystalline solid in that they preserve long-range order in spite of atomic movement. As a consequence, heat transfer is due both to electronic movement and to lattice vibrations, which can be described in terms of phonons. Since electrons take part in both electric and thermal transport, the relative importance of the lattice and electronic contributions to the thermal conductivity depends on the value of the electric conductivity 𝜎. In metals, where thermal conduction is dominated by electrons, both conductivities are related by the Wiedemann-Franz law, 𝜅𝜎=𝐿𝐿𝑇, (2.2) where 𝐿𝐿is known as the Lorenz number. In the framework of free-electron theory, 𝐿𝐿has a universal value of 2.44⋅10−􀁵 􀃶􀃃 􀃪􀁹. In practice, however, there are values of 𝐿𝐿which afford a better fit to experimental data for each particular metal [74]. It must also be noted that the Wiedemann-Franzlaw can be violated in the nanoscale, either because of the important role played by fluctuations [75] or when the electron gas is close to a phase transition [76]. The case of semiconductors is more complex as both contributions to the thermal conductivity must be taken into account. A detailed study by Shanks et al. [77] concludes that the thermal conductivity of Si up to 1000Kcan be attributed almost exclusively to phonons; likewise, Kugman and Stegmeier [78] point out that the contribution of charge carriers to the thermal conductivity of InP is negligible at least up to 800K. However, this is not necessarily the case for nanowires. A theoretical study based on the Boltzmann transport equation [61] predicts the existence of a crossover, at a width between approximately 5 and 10nmdepending on the material, below which the electronic contribution becomes dominant. The study of this part of the total thermal conductivity is closely tied to the study of electric transport. Simple approximations like the Wiedemann-Franz law can be used to explain experimental results, but in order to achieve predictive power ab-initio techniques are required, which at this point are still very limited in the number of atoms they can handle. For this reason, the work contained in this chapter is limited to the study of the lattice contribution to 𝜅. Phonons are spin-1bosons, and accordingly their occupation numbers follow the Bose-Einstein distribution at thermal equilibrium. Computational techniques that take into account their quantum character will be employed in later chapters. Nevertheless, when the temperature is high enough, the 14 2.2. Intermolecular potential internal energy of a boson gas is so large that the effects introduced by their indistinguishability become minor by virtue of the fact that there are few bosons in each quantum state, a situation known as the dilute limit. An estimate of the temperature at which this happens can be obtained from the rather crude Debye model, in which all phonons have linear dispersion relations and a frequency cutoff 𝜔𝐷is introduced in order to ensure the correct number of vibrational modes. Denoting Boltzmann’s constant and the reduced Plank constant by 𝑘𝐵and ℏrespectively, it is easy to show that when 𝑇>𝑇𝐷=ℏ𝜔𝐷/𝑘𝐵, the Debye temperature, the results of the Debye model approximate those of the classical gas of harmonic oscillators. For Si and InP, the values of 𝑇𝐷are 645Kand 425K, respectively [74]. From a computational point of view, treating a system classically has some important advantages, because the available methods are less time-consuming and thus allow larger sets of atoms to be considered. However, the Debye temperatures mentioned in the previous paragraph are well above room temperature, giving the impression that such treatment would not lead to useful results. Fortunately, the vibrational modes most relevant for thermal conduction lie well below the Debye frequency and are, therefore, well populated at much lower temperatures — around 150Kfor Si, according to Ref. 79. Thus, a classical simulation method was chosen to calculate the thermal conductivity of InP nanowires in the temperature range between 100and 700K. In particular, after a revision of the literature, an MD approach was chosen instead of a Montecarlo method, more adapted to the modelling of particle diffusion. MD methods are based on the numerical integration of Newton’s equations of motion and the analysis of the resulting trajectories, and as such they require three ingredients: an intermolecular potential, an integration method and an expression of the variable under study in terms amenable to classical mechanics. 2.2. Intermolecular potential As regards the first of these elements, there are plenty of potentials in the literature, ranging from the simplest ones (Lennard-Jones or hard spheres, for instance) to those with hundreds of parameters (such as ReaxFF [80]). The functional form of these potentials usually comes from theoretical insights about the dominant interactions in the systems they try to describe, but the precise values of their parameters are often fitted so that they afford predic- 15 2. MD predictions of the thermal conductivity of thin InP nanowires 𝑗𝑄=1𝑉⎡⎢⎢⎣􀈪 𝑖𝑣𝑖𝜀𝑖+12􀈪 􀊂𝑖,𝑗􀊅∈􀂝􀂎􀂖􀂟􀂠𝑟𝑖𝑗􀊂𝐹𝑖𝑗⋅𝑣𝑖􀊅+􀈪 􀊂𝑖,𝑗,𝑘􀊅∈􀂡􀂟􀂖􀂝􀂙􀂒􀂡􀂠𝑟𝑖𝑗􀊂𝐹𝑗𝑖𝑘⋅𝑣𝑗􀊅⎤⎥⎥⎦(2.12a) 𝜀𝑖=12𝑚𝑖􀉤𝑣𝑖􀉤􀁯+12􀈪 𝑗􀉥􀊂𝑖,𝑗􀊅∈􀂝􀂎􀂖􀂟􀂠𝑉(􀁯) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅+16􀈪 𝑗,𝑘􀉥􀊂𝑖,𝑗,𝑙􀊅∈􀂡􀂟􀂖􀂝􀂙􀂒􀂡􀂠𝑉(􀁰) 𝑖𝑗𝑘 􀊂𝑟𝑖𝑗,𝑟𝑖𝑘􀊅.(2.12b) The fact that no temperature gradient needs to be applied gives equilibrium methods a certain theoretical appeal. They are also useful when studying anisotropic systems, since (2.8) can be straightforwardly generalised to any component of the conductivity tensor. However, they demand very long equilibration times and, even so, the precision they yield is quite modest (∼20% uncertainty). On a more fundamental level, there are several possible definitions of heat current in addition to Eq. (2.11) and, as discussed in Ref. 92, each of them affords a different autocorrelation function. This is a reflection of the aforementioned problems with the concept of heat. Moreover, in order to obtain physically meaningful results, it seems necessary to filter out the highfrequency components of the autocorrelation function [92] using a somewhat arbitrary cutoff frequency. An alternative to equilibrium methods is offered by HNEMD [93]. In this framework, a fictitious force 𝐹𝑒is applied to the system, chosen in such a way that the Green-Kubo relation (2.8) takes a diagonal form and 𝜅can be shown to be proportional to 𝑙𝑖𝑚𝐹𝑒→􀁭􀈘𝑗(𝑧) 𝑄􀈋/𝐹𝑒. Even though they are mathematically complex and require especial integration schemes [94], HNEMD methods are the best alternative available in terms of efficiency [95]. However, their generalisations to multicomponent systems and many-body potentials have only been developed recently [95, 96] and cannot be considered as proven as more traditional methods. In the light of the shortcomings of Green-Kubo and HNEMD methods, a direct non-equilibrium approach was deemed as preferable. To keep the nanowire in a non-equilibrium steady state, two areas of the nanowire must be defined as thermostats. From that point, two routes are possible: either the temperatures of those thermostats can be kept fixed and the thermal current calculated using an expression such as Eq. (2.12), or the energy can be kept fixed and the temperature gradient calculated instead. The second option offers the advantage of being independent of any particular expression of the thermal current, so it was the one implemented in this case. Figure 2.2 22 2.4. Calculation of the thermal conductivity Figure 2.2 Scheme of a nanowire in a steady state. shows a schematic drawing of a nanowire in this situation. The system was divided in a number 𝑛𝑠of segments of equal length along its long axis, so that the 𝐼-th segment extended from 𝑧=(𝐼−1)𝐿 𝑛𝑠to 𝑧=𝐼𝐿 𝑛𝑠. The temperature of each of these segments was computed using the equipartition theorem 𝑇𝐼(𝑛𝛥𝑡)=1 𝑀𝑛 􀈪 𝑘=𝑛−𝑀 ∑  𝑟𝑖(𝑘𝛥𝑡)∈𝐼𝑚𝑖􀉤𝑣𝑖(𝑘𝛥𝑡)􀉤􀁯 3𝑘𝐵∑  𝑟𝑖(𝑘𝛥𝑡)∈𝐼1,(2.13) which clearly implies a hypothesis of approximate local equilibrium among the atoms in each segment. It must be mentioned that a small number of studies, such as Ref. 97, apply a “quantum correction” to this temperature, based on a Debye model and the Bose-Einstein distribution. It was judged that this correction is based precisely on the application of the equipartition theorem to a quantum problem for which it is known not to hold. On the other hand, MD gives rise to completely classical velocity distributions corresponding to a thermodynamic temperature which matches the prediction of that theorem. Moreover, the Debye model is merely a rather crude approximation to reality. For these reasons, such correction was not applied here. In any case, it has 23 2. MD predictions of the thermal conductivity of thin InP nanowires never been shown to yield better explanations of experimental data, and studies which have assessed its applicability by comparing it with fully quantum methods strongly discourage its use [98]. As depicted in Fig. 2.2, two thermostated plates were placed at 𝑧=𝐿/4and 𝑧=3𝐿/4(hot and cold, respectively). At each time step, an amount of energy 𝛥𝐸was added to the atoms inside the thermostat on the left, and the same amount was removed from those in the thermostat on the right. If, starting from equilibrium at temperature 𝑇, this procedure is repeated during enough time steps, a steady state is reached in which the average temperature of the nanowire is still 𝑇, but a constant temperature difference exists between those segments closer to the hot thermostat and those further from it. Since in such a state the heat flux along the nanowire must compensate the energy added by the hot plate (or removed by the cold plate) per unit time and area, 𝑗(𝑧) 𝑄=𝛥𝐸 2𝐴𝛥𝑡.(2.14) A factor 2is present in the denominator of this expression because heat can flow in two directions owing to the use of periodic boundary conditions (PBC) along the 𝑂𝑍axis. Therefore, each segment between the plates had an equivalent outside this region, and the simulation generated twice the amount of data it would if PBC were not applied. The temperature gradient ∇𝑇was calculated by a linear fit of the temperatures of the segments, and its stability through a long number of time steps was used as the criterion by which to determine when the system had reached the desired steady state. In the immediate neighbourhoods of the thermostats there are non-linearities in the temperature profile, so those segments were excluded from the fit. The accuracy of this approach has been favourably compared with that of Green-Kubo methods by several authors [42, 99]. Many procedures to add and remove energy from the atoms in the thermostated regions can be devised, based on the plethora of MD thermostats proposed in the physical literature. Taking into account that the precise reproduction of a Maxwell-Boltzmann distribution is not critical, a simple velocity rescaling thermostat was chosen, as usual in this kind of work [42, 100]. Let 𝑖 run over the particles in a thermostat and 𝑣𝑐𝑚 =∑𝑖𝑚𝑖𝑣𝑖/∑𝑖𝑚𝑖be the velocity of its centreof mass. At eachtime step, the followingtransformation was applied: 24 2.5. Characterisation of the phonon densities of states 𝑣′𝑖=𝑣𝑐𝑚+𝛼􀊂𝑣𝑖−𝑣𝑐𝑚􀊅(2.15a) 𝛼=􀇿1± 𝛥𝐸 𝐸𝑘𝑖𝑛,𝑅 (2.15b) 𝐸𝑘𝑖𝑛,𝑅 =12􀈪 𝑖𝑚𝑖􀉤𝑣𝑖􀉤􀁯−12􀊄􀈪 𝑖𝑚𝑖􀊇􀉤𝑣𝑐𝑚􀉤􀁯.(2.15c) In Eq. (2.15b), the positive sign refers to the hot thermostat and the negative sign to the cold plate. It is easy to check that this transformation conserves the velocity of the centre of mass and that it changes the kinetic energy by the desired amount. To complete the description of the simulation method, it remains to specify the initial conditions. These were extracted from an equilibrium simulation with the same systems and potential, 𝛥𝑡=0.01psand a total simulation time of 10ns(10􀁳steps), enough to stabilise the nanowires at any of the temperatures of interest using the Berendsen thermostat [101], which rescales all the velocities in a gradual fashion until the final temperature 𝑇𝑓is reached: 𝑣′𝑖=􀉾1+𝛥𝑡 𝜏􀊄𝑇𝑓 𝑇−1􀊇􀊁􀁸 􀁹𝑣𝑖.(2.16) 𝜏determines the speed at which the temperature is modified: the larger it is, the longer the simulation must be and the smaller the probability that the system explodes. A value 𝜏=1pswas used for this work. After reaching 𝑇𝑓, the nanowires were simulated without any thermostat for an additional 1ns to eliminate any residual effect of velocity rescaling. 2.5. Characterisation of the phonon densities of states Comparison of the phonon densities of states (DOS) between different nanowires can help analyse the effect of nanowire width on thermal conductivity. Unfortunately, a priori information about phonons is not directly available from MD simulations, which are based on atoms. Therefore, the DOS must be extracted from an analysis of the trajectories. Let us consider a set of 𝑁atoms with 3𝑁vibrational modes, with frequencies {𝜔𝑚}􀁰𝑁 𝑚=􀁮, around a minimum of the potential so that for energies close to the bottom of that potential well each of the velocities can be expressed in a harmonic 25 2. MD predictions of the thermal conductivity of thin InP nanowires form, 𝑣𝑖(𝑡)=ℜ􀊈∑􀁰𝑁 𝑚=􀁮  𝐴𝑖,𝑚𝑒−𝑗𝜔𝑚𝑡􀊋. Hence, the statistical average of its time autocorrelation function has the form 􀈗𝑣𝑖(0)⋅𝑣𝑖(𝑡)􀈊=􀁰𝑁 􀈪 𝑚=􀁮,𝑛=􀁮􀈘ℜ􀊈 𝐴𝑖,𝑚𝑒−𝑗𝜔𝑚𝑡􀊋⋅ℜ􀊈 𝐴𝑖,𝑛􀊋􀈋= =12ℜ⎧⎪⎪⎪⎨⎪⎪⎪⎩􀁰𝑁 􀈪 𝑚=􀁮𝑒−𝑗𝜔𝑚𝑡􀊄􀁰𝑁 􀈪 𝑛=􀁮􀈘 𝐴𝑖,𝑚⋅ 𝐴𝑖,𝑛+ 𝐴𝑖,𝑚⋅ 𝐴∗𝑖,𝑛􀈋􀊇 􀉙􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀉚􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀅾􀉛 =∶𝑐𝑚 ⎫⎪⎪⎪⎬⎪⎪⎪⎭,(2.17) so its Fourier transform is proportional to ∑􀁰𝑁 𝑚=􀁮𝑐𝑚[𝛿(𝜔−𝜔𝑚)+𝛿(𝜔+𝜔𝑚)], which is non-zero at the same positions as the phonon DOS, but is modulated by an occupancy factor. In practice, true mechano-statistical averages are not available in MD simulations, so they have to be approximated by averages over time and over particles. Moreover, MD is not a purely harmonic formalism, and anharmonic effects will introduce temperature-dependent variations in this result. Accordingly, instead of 𝛿functions more or less broad peaks will be observed. In any case, a reasonable idea about the form of the phonon DOS can be obtained by studying the squared modulus of the Fourier transform of the normalised velocity autocorrelation function 𝑍(𝑡),i.e., |ℱ[𝑍(𝑡),𝜔]|􀁯=􀉧ℱ􀉾􀈗𝑣𝑖(0)⋅𝑣𝑖(𝑡)􀈊 􀈗𝑣𝑖(0)⋅𝑣𝑖(0)􀈊;𝜔􀊁􀉧􀁯.(2.18) It is even possible to go further and calculate, by similar methods, the phonon dispersion relation 𝜔􀊂𝑘􀊅. From a theoretical point of view, this can be accomplished by taking the autocorrelation function of a projection of the velocities on the appropriate plane wave, 𝜈 𝑘(𝑡)=∑𝑖𝑣𝑖(𝑡)𝑒−𝑗 𝑘⋅ 𝑟𝑖(𝑡). In practice, however, this is computationally prohibitive, especially if a fine enough 𝑘-point grid is to be sampled in order to compute group velocities or similar variables. For this reason, examples of this technique have only been found in the literature for simple pair potentials [102, 103]. 2.6. Computational details The equilibrium simulation used to generate sets of initial conditions, the non-equilibrium simulation itself and the post-processing part were implemented as Fortran 90 programs for efficiency. The most time-consuming parts 26 2.7. Results and discussion of the code, such as the evaluation of 𝑉and its derivatives, where parallelised using OpenMP, a set of directives for multiprocessing on shared-memory platforms. To this end, the systems were divided in as many segments as processors were available, so that the forces on the particles of each segment could be calculated, and their dynamic properties updated, in parallel. Since the Branício-Rino potential is short-ranged, neighbour tables were used in order to avoid the need to re-evaluate cutoffs at each time step. Analytic expressions for the forces where derived from Eqs. (2.4) and implemented:  𝑓𝑖𝑗 =−𝑟𝑖𝑗𝑑𝑉(􀁯) 𝑖𝑗 𝑑𝑟𝑖𝑗 =𝑟𝑖𝑗⎧⎪⎨⎪⎩𝜂𝑖𝑗 𝑟𝑖𝑗 􀊄𝜎𝑖+𝜎𝑗 𝑟𝑖𝑗 􀊇𝜂𝑖𝑗 +􀊄1 𝑟𝑖𝑗 +1 𝑟􀁮𝑠􀊇𝑍𝑖𝑍𝑗 𝑟𝑖𝑗 𝑒−𝑟𝑖𝑗 𝑟􀁸𝑠 −􀊄4 𝑟𝑖𝑗 +1 𝑟􀁱𝑠􀊇􀁮 􀁯􀊂𝛼𝑖𝑍􀁯 𝑗+𝛼𝑗𝑍􀁯 𝑖􀊅 𝑟􀁱 𝑖𝑗 𝑒−𝑟𝑖𝑗 𝑟􀁻𝑠 −6 𝑟𝑖𝑗𝑤𝑖𝑗 𝑟􀁳 𝑖𝑗 ⎫⎪⎪⎬⎪⎪⎭  𝑓𝑖𝑗𝑘 =−∇𝑖𝑉(􀁰) 𝑖𝑗𝑘 =− 𝑓𝑗𝑘𝑖− 𝑓𝑘𝑖𝑗  𝑓𝑗𝑘𝑖 =−∇𝑗𝑉(􀁰) 𝑖𝑗𝑘 =− 𝐴𝑋𝜁 􀊂𝑟𝑖𝑗−𝑟􀁭􀊅􀁯𝑟𝑖𝑗−2𝐴 𝑌𝑟𝑖𝑗 􀊂𝑟𝑖𝑗𝑐𝑜𝑠𝜃𝑖𝑗𝑘−𝑟𝑖𝑘􀊅  𝑓𝑘𝑖𝑗 =−∇𝑘𝑉(􀁰) 𝑖𝑗𝑘 =− 𝐴𝑋𝜁 (𝑟𝑖𝑘−𝑟􀁭)􀁯𝑟𝑖𝑘−2𝐴 𝑌𝑟𝑖𝑘 􀊂𝑟𝑖𝑘𝑐𝑜𝑠𝜃𝑖𝑗𝑘−𝑟𝑖𝑗􀊅 𝐴=𝐵𝑖𝑗𝑘𝑒𝑥𝑝􀊄𝜁 𝑟𝑖𝑗−𝑟􀁭+𝜁 𝑟𝑖𝑘−𝑟􀁭􀊇𝑋 𝑌 𝑌=1+𝐶𝑋􀁯 𝑋=𝑐𝑜𝑠𝜃𝑖𝑗𝑘−𝑐𝑜𝑠𝜃􀁭. (2.19) The results presented in this chapter took about 2500hof CPU time at the Galician Supercomputing Centre (CESGA). 2.7. Results and discussion The nanowires for this study were constructed by cutting an hexagonal prism out of zinc-blende bulk InP with the [111]crystallographic direction — the diagonal of the conventional cubic unit cell — as its axis. Alternatively, they can be thought of as built by piling layers of close-packed spheres following a periodic ABCABC… pattern, and then placing a two-atom {In,P}basis at the centre of each sphere with the In-P bond perpendicular to the corresponding layer. These three inequivalent layers are shown, for a particular diameter, 27 2. MD predictions of the thermal conductivity of thin InP nanowires Figure 2.3 Constructive block for nanowires with six radial layers, seen from three different directions: a) [111](long axis of the wire); b) [110]; c) [100]. Orange intersections are In atoms; violet intersections represent P. in Fig. 2.3. The equilibrium In-P distance in the bulk material is 2.54 A, so contiguous layers are separated by 3.39 A. On the other hand, the minimum in-layer interatomic distance equals the distance between the centres of two faces of the conventional unit cell, 4.15 A. Hence, the radius of the smallest circumference that encloses all the atoms in a nanowire comprising 𝑛𝑟radial layers (excluding the fixed atoms) is 4.15(𝑛𝑟−1)A. The cross-sectional area of the thermally conducting part of such a wire is 𝐴=0.447(𝑛𝑟−1)􀁯nm􀁯. Thin wires are more interesting with regard to surface effects; in addition, there is an upper bound on the diameter of a tractable nanowire owing to the quadratic dependence of the number of atoms on it. According to these criteria, nanowires with 2to 7radial layers of mobile atoms, and diameters 0.83,1.66, 2.49,3.32,4.15and 4.97nm, were chosen. The case of only one mobile radial layer was excluded because it does not have a well-defined diameter. The numbers of atoms in the simulated nanowires ranged from 37950to 94650. The rate of energy addition and removal 𝛥𝐸/𝛥𝑡was another parameter which required a careful choice. It had to be small enough that it still made 28 2.7. Results and discussion sense to refer to the result of the calculation as the thermal conductivity at temperature 𝑇in spite of the difference in temperature (𝛥𝑇) induced between the thermostats, but not so small that 𝛥𝑇was masked by fluctuations in the “instantaneous” temperature of the system. Moreover, it must be scaled proportionally to thenumber of mobile atomsin eachthermostatif 𝛥𝑇is tobe roughly independent of the diameter. Based on these considerations, 𝛥𝐸=0.01eVwas chosen for the thinnest nanowire, which yielded values of 𝛥𝑇around 10K. Two related parameters are the width of each thermostated plate, 𝛿, and the number of segments around each of them which should be excluded from the linear fit. As regards the former, the results proved rather insensitive to the precise choice of 𝛿, which was finally set to 10nmto improve convergence by adding/removing less energy to/from each individual atom. The latter problem was solved by widening the excluded region until a point was reached where ∇𝑇remained stable. This happened quite soon, for a width of merely 5nm. The value of 𝜅derived from the simulation depends quite strongly on the length of the simulation box as long as the latter is comparable to the mean free path (MFP) or to the wavelength of phonons involved in thermal conduction. Its effect can be treated in a simplistic manner as follows [42]. Let 𝑙∞be the MFP of phonons in a particular state for an infinite nanowire, and 𝑙𝐿be the same variable for a wire of length 𝐿. If scattering by the ends of the wire is assumed to be independent from every other scattering mechanism, the total scattering probability per unit length (𝑙−􀁮 𝐿) can be approximated by the sum of 𝑙−􀁮 ∞and 􀁱 𝐿(since the average distance from a random point along the nanowire to the closest thermostat is 𝐿/4). In elementary kinetic theory, the contribution of a vibrational mode to 𝜅is proportional its MFP. Thus, for some constant 𝑏, 1 𝜅𝐿=1 𝜅∞+𝑏𝐿.(2.20) In principle, this expression could be used to extrapolate the true value of the thermal conductivity, 𝜅∞, from a set of results (𝜅𝐿) suffering from size effects, using a simple linear fit. However, its applications in the literature have never been too successful, either because of the huge uncertainties in the extrapolated𝜅−􀁮 ∞[99] orbecauseit canyield unphysical, andeven negative, values [104]. Some authors have obtained better results modelling the dependence of 𝜅𝐿on 𝐿as linear. In any case, it seems clear that this dependence is not so simple. For the InP nanowires investigatedin this work, simulationboxes comprising from 29 2. MD predictions of the thermal conductivity of thin InP nanowires Figure 2.4 Typical steady-state temperature profile. For this figure, the nanowire was divided in 40segments, instead of the usual 20, to show a more detailed picture of non-linear regions. Each point in the plot is the average of two segments, one to the right and one to the left of the hot thermostat, equivalent owing to the application of PBC. 270 280 290 300 310 320 330 T(K) 75to 900layers along the longitudinal axis were tried, which revealed that a fit to Eq. (2.20) is inconclusive, as it results in uncertainties of up to 400%in the ordinate at the origin. As a matter of fact, 𝜅seems to remain constant, within the limits of computational uncertainty, if more than about 200layers are included in the box. 225layers were always used for the final calculations. The Pearson deviation coefficient of temperature, as calculated using the equipartition theorem, is inversely proportional to the square root of the number of atoms used. This limits the number of segments in which the nanowire should be conceptually split. 20segments, each one comprising between 1900 and 4700atoms depending on the diameter, were settled on as a good compromise between a precise temperature and a sufficient number of data points for the linear fit. Figure 2.5 shows the temporal evolution of the temperature gradient thus calculated, from the instant when energy began to be moved along the nanowire at equilibrium to a point where a steady-state was reached. Thecriterionusedtoidentifysuchpointwasthat𝜕𝑇/𝜕𝑧remainedstablewithin a1%for 1ns. After this, each simulation was run for a further 1ns; this time was divided in 10subintervals, each of which yielded a different value of 𝜕𝑇/𝜕𝑧. From the sample of 10values, their mean was taken as the best estimator of the thermal gradient and their standard deviation of the sample 30 2.7. Results and discussion Figure 2.5 Representative example of the evolution with simulation time of the average temperature gradient in a nanowire. The steady-state profile for the same simulation is shown in Fig. 2.4. 0 100 200 300 400 500 600 t(ps) -0.06 -0.04 -0.02 0.00 ∂T ∂z K m ( ) mean as the uncertainty, which was then propagated to 𝜅=􀉦􀊂𝜕𝑇/𝜕𝑧􀊅−􀁮𝑗(𝑧) 𝑄􀉦.(2.21) The uncertainty 𝑠􀊃𝜕𝑇 𝜕𝑧􀊆is mostly insensitive to a change in the number of temporal subintervals, but falls when the total simulation time is increased, down to a limit. Its evolution is exemplified in Fig. 2.6; the fact that it stabilises under 10%, considered a good value in the literature [42, 99], supports the choice of parameters in this work. However, this estimator of uncertainty was not considered reliable enough to attach an individual uncertainty to each result, as there are many assumptions implicit in the method whose contributions to the combined uncertainty would be difficult to ascertain. As mentioned in previous sections, thermal conductivity calculations were performed for nanowires with diameters 𝑑between 1.66and 4.97nm at temperatures between 100and 700K. Figure 2.7 shows the results for 𝑑=1.66nmand 𝑑=4.15nm. For the smallest diameter, 𝜅(𝑇)falls globally from 2.3W/(mK)at 100Kto 1.5W/(mK)at 700K, but shows a local maximum of around 2.25 W/(mK)between 300and 400 K. In contrast, the thermal conductivity of the nanowire with 𝑑=4.15nmis almost flat in the range 100−500 Kand falls monotonically after that, from around 31 2. MD predictions of the thermal conductivity of thin InP nanowires 60. Harrison, W. A. Electronic Structure and the Properties of Solids (Dover, New York, 1989). 61. Mingo, N. & Broido, D. A. Phys. Rev. Lett. 93, 246106 (2004). 62. Mingo, N. Appl. Phys. Lett. 84, 2652 (2004). 63. Branício, P. S. & Rino, J. P. Phys. Stat. Sol. (b) 244, 331 (2007). 64. Vashishta, P., Kalia, R. K., Rino, J. P. & Ebbsjö, I. Phys. Rev. B 41, 12197 (1990). 65. Shimojo, F., Ebbsjö, I., Kalia, R. K., Nakano, A., Rino, J. P. & Vashishta, P. Phys. Rev. Lett. 84, 3338 (2000). 66. Rino, J. P., Chatterjee, A., Ebbsjö, I., Kalia, R. K., Nakano, A., Shimojo, F. & Vashishta, P. Phys. Rev. B 65, 195206 (2002). 67. Branício, P. S., Kalia, R. K., Nakano, A., Rino, J. P., Shimojo, F. & Vashishta, P. Appl. Phys. Lett. 82, 1057 (2003). 68. Rino, J. P. & Branício, P. S. Phys. Stat. Sol. (b) 244, 239 (2007). 69. Lieb, E. H. & Yngvason, J. Phys. Rep. 310, 1 (1996). 70. Carathéodory, C. Math. Ann 67, 355 (1909). 71. Buchdahl, H. A. The Concepts of Classical Thermodynamics (Cambridge University Press, Cambridge, 1966). 72. Boyling, J. B. Proc. Roy. Soc. London A 329, 35 (1972). 73. Grandy, W. T. Jr. Found. Phys. 34, 21 (2004). 74. Kittel, C. Introduction to Solid State Physics 8th Edition (Wiley, 2004). 75. Vavilov, M. G. & Stone, A. D. Phys. Rev. B 72, 205107 (2005). 76. Tanatar, M. A., Paglione, J., Petrovic, C. & Taillefer, L. Science 316, 1320 (2007). 77. Shanks, H. R., Maycock, P. D., Sidles, P. & Danielson, G. C. Phys. Rev. 130, 1743 (1963). 78. Kudman, I. & Steigmeier, E. F. Phys. Rev. 133, 1665 (1964). 79. Ju, Y. S. Appl. Phys. Lett. 87, 153106 (2005). 80. Van Duin, A. C. T., Dasgupta, S., Lorant, F. & Goddard III, W. A. J. Phys. Chem. A 105, 9396 (2001). 81. Rey, C., Gallego, L. J., García-Rodeja, J., Alonso, J. A. & Iñiguez, M. P. Phys. Rev. B 48, 8253 (1993). 38 References 82. García-Rodeja, J., Rey, C., Gallego, L. J. & Alonso, J. A. Phys. Rev. B 49, 8495 (1994). 83. Xiao-Kun, G. & Bing-Yang, C. Chin. Phys. 16, 3777 (2007). 84. N. Yang, G. Z. & Li, B. Nano Lett. 8, 276 (2007). 85. Gomes, C. J., Madrid, M., Goicochea, J. V. & Amon, C. H. J. Heat Transfer 128, 1114 (2006). 86. Chen, G. Y., Stolojan, V., Cox, D. C., Giusca, C. & Silva, S. R. P. in IEEE Conference on Emerging Technologies - Nanoelectronics (2006), 376. 87. Yang,W.,Araki,H.,Kohyama, A.,Thaveethavorn,S.,Suzuki,H.&Noda, T. Mater. Lett. 58, 3145 (2004). 88. Wang, S., Liang, X. & Ohara, T. J. Appl. Phys. 105, 014316 (2009). 89. Swope, W. C., Andersen, H. C. & amd K. R. Wilson, P. H. B. J. Chem. Phys. 76, 637 (1982). 90. Van Zon, R. CHM1464: Foundations of Molecular Dynamics, course notes Booklet avaliable online at the University of Toronto web site http:// www.chem.utoronto. ca /~rzon/simcourse/notes .html. Retrieved on 2012-04-06. 2005. 91. Carrete, J., Varela, L. M. & Gallego, L. J. Physica A 27, 6752 (2008). 92. Guajardo-Cuéllar, A., Go, D. B. & Sen, M. J. Chem. Phys. 132, 104111 (2010). 93. Evans, D. J. &Morriss,G. P.Statistical Mechanics of NonEquilibrium Liquids 1st ed. (Academic Press, London, 1990). 94. G, G. P., Ely, J. F., McCabe, C. & Isbister, D. J. J. Chem. Phys. 122, 094114 (2005). 95. Mandadapu, K. K., Jones, R. E. & Papadopoulos, P. J. Chem. Phys. 133, 034122 (2010). 96. Mandadapu, K. K., Jones, R. E. & Papadopoulos, P. J. Chem. Phys. 130, 204106 (2009). 97. Huang, X., Huai, X., Liang, S. & Wang, X. J. Phys. B 42, 095416 (2009). 98. Turney, J. E., McGaughey, A. J. H. & Amon, C. H. Phys. Rev. B 79, 224305 (2009). 99. Zhou, X. W., Aubry, S., Jones, R. E., Greenstein, A. & Schelling, P. K. Phys. Rev. B 79, 115201 (2009). 39 2. MD predictions of the thermal conductivity of thin InP nanowires 100. Jund, P. & Jullien, R. Phys. Rev. B 59, 13707 (1999). 101. Berendsen, H. J. C., Postma, J. P. M., van Gunsteren, W. F., Dinola, A. & Haak, J. R. J. Chem. Phys. 81, 3684 (1984). 102. Papanicolaou, N. I., Lagaris, I. E. & Evangelakis, G. A. Surf. Sci. 337, L819 (1995). 103. Heino, P. Eur. Phys. J. B 60, 171 (2007). 104. Yoo, Y.-G., Car, R., Srolovitz, D. J. & Scandolo, S. Phys. Rev. B 70, 012302 (2004). 105. Aliev, S. A., Nashelskii, A. Y. & Shalyt, S. S. Sov. Phys. Solid State 7, 1287 (1965). 106. Balandin, A. & Wang, K. L. Phys. Rev. B 58, 1544 (1998). 107. Adu, K. W., Gutiérrez, H. R., Kim, U. J., Sumanasekera, G. U., & Eklund, P. C. Nano Lett. 5, 409 (2005). 40 3Influence of the interatomic potential on MD calculations of thermal conductivity: comparison for GaAs, InAs and InP nanowires Aunt Martha: For a gallon of elderberry wine, I take one teaspoon full of arsenic, then add half a teaspoon full of strychnine, and then just a pinch of cyanide. Mortimer Brewster: Hmm. Should have quite a kick. Arsenic and Old Lace Frank Kapra 3.1. Introduction In Chapter 2, MD simulations were used to calculate the thermal conductivity of hexagonal InP nanowires. One of the relevant conclusions was that an enhancement of 𝜅is obtained when the diameter is reduced beyond a certain limit. However, such enhancement is small enough for its statistical significance to be questionable, given the uncertainty in the data. Therefore, it is important to assess the reliability of the diverse elements which can affect this calculation. One of the most complicated choices is the interatomic potential, 41 3. Influence of the potential on MD thermal conductivity as generally none of them can be expected to give good results for every property of the system under study, and transferability can be difficult to evaluate a priori. As mentioned previously, most theoretical and computational work on the thermalconductivitiesofnanowireshasbeenlimitedtoSi[36,38,39,41].In the most salient exception, predictions of the room-temperature thermal conductivities of nanowires of the zinc-blende-structured semiconductors CdTe, ZnTe, ZnSe, ZnS, InSb, InAs, GaSb, GaAs, AlSb and InP were obtained by Mingo and Broido [61] from phonon dispersion relations that were calculated atomistically using a Harrison potential [60] while fitting a parameter related to the specularity of the boundary (see also Refs. 62, 108 and 109, as well as the more precise definition of the role of specularity in Section 4.5). However, the results extrapolated from Mingo and Broido’s prediction [61] are an order of magnitude smaller than those discussed in Chapter 2 and based on the Branício- Rino potential [63]. Mingo and Broido also found that for binary semiconductorsofagiventype(III-VorII-IV),theratio𝜅􀂏􀂢􀂙􀂘/𝜅􀂛􀂎􀂛􀂜between the thermal conductivities of the bulk and of nanowires of a given diameter increased with the mass ratio 𝑟of the components, so that for GaAs (𝑟=1.07), InAs (𝑟=1.53) and InP (𝑟=3.71)𝜅􀂏􀂢􀂙􀂘/𝜅􀂛􀂎􀂛􀂜increased in the order GaAs<InAs<InP. In the work described here the thermal conductivities of GaAs, InAs and InP nanowires at 𝑇=300Kwere computed by direct MD simulations of the kind describedin the previous chapter, in eachcase obtainingresults both with the classical Harrison potential [60] as parameterised by Mingo and Broido [61], and also with another, more elaborate potential. For GaAs and InAs the Abell-Tersoff potential recently parameterised by Hammerschmidt et al. [110] for the description of GaAs and InAs nanostructures was used, and for InP the choice wasagaintheBranício-Rinopotential[63].Theaims of thesecalculations were twofold: firstly, to comparethe theoretical predictions ofMingo and Broido [61] with the results of MD simulations using the same Harrison potential, so asto check, in particular, whether the above-noteddiscrepancy between Ref. 61 and Chapter 2 was due to the use of different potentials or different methods; secondly, toinvestigate whether for GaAsand InAsnanowires a similar discrepancy emerged between Mingo and Broido’s [61] Harrison-based theoretical results and MD results obtained with the Abell-Tersoff/Hammerschmidt potential. 42 3.2. Details of the MD simulations and of the model potentials 3.2. Details of the MD simulations and of the model potentials The ingredients used for MD calculations in this work are basically the same as in Chapter 2: a direct non-equilibrium method [42], hexagonal nanowires cut along the [111]direction of the zinc-blende bulk, the velocity Verlet integration algorithm [89] and rigid boundary conditions. Regarding the latter, it should be noted that the theoretical results of Mingo and Broido [61] were also obtained by imposing frozen boundary conditions on the wires. Each nanowire occupied a large supercell with periodic boundary conditions in the 𝑧direction so as to make the wire endless. The length of this supercell, 𝐿, was chosen so as to avoid aliasing phenomena that might suppress important contributions to the thermal conductivity from long-wavelength phonons. To this end, simulations using nanowires of a fixed diameter and lengths of up to 1800atomic layers were ran, which allowed the determination of lengths big enough to ensure that any loss of thermal conductivity resulting from the finite value of 𝐿was within the uncertainty of the simulation results: 97.2nmfor GaAs, 104.8nmfor InAs and 76.2nmfor InP. A fit of the dependence of thermal conductivity on supercell length to Eq. (2.20) was attempted as suggested by Schelling et al. [42], but again the results were not satisfactory. This is qualitatively in line with more recent results from the literature [99, 111–113], which call into question the linear extrapolation procedure. To calculate the temperature gradient 𝜕𝑇/𝜕𝑧, the nanowire was notionally divided into 20segments, their kinetic temperatures were averaged over 10􀁴 time steps after the steady state had been reached, the four segments containing the thermostats were discarded (with 20segments, each thermostat is centred at the boundary between two segments), and a linear regression of segment temperature on the distance of the segment midpoint from the hot plate was performed. The thermal conductivity at the centre of the cell (i.e. at the mean temperature of the two thermostats) was obtained using Eq. (2.21). Due to their computational demands, these MDsimulations were necessarily restricted to nanowires of small diameter: the unconstrained parts of the wires with 4,5,6and 7mobile layers surrounding the central row of atoms had diameters of respectively 2.57,3.42,4.28and 5.13nm(GaAs) and 2.38, 3.17,3.97and 4.76nm(InAs), and those of the InP wires with 3,4,5and 6 unconstrained layers around the central row had diameters of 2.49,3.32,4.15 and 4.97nmrespectively. The total numbers of atoms, including those of the 43 3. Influence of the potential on MD thermal conductivity Table 3.1 Parameters of the Harrison potential, copied from Ref. 61. InP InAs GaAs 𝐶􀁭(eV)47.38 42.13 42.04 𝐶􀁮(eV)0.715 0.650 0.826 fixed layers, ranged from 18200to 126200for GaAs and InAs, and from 37950 to 94650for InP. The Harrison potential [60], which was used for GaAs, InAs and InP, computes the total potential energy of the system as the sum of quadratic terms describing the interactions between nearest-neighbour pairs and triplets, 𝑉=𝐶􀁭 2𝑟􀁯 􀁭􀈪′ 􀊂𝑖,𝑗􀊅􀊂𝑟𝑖𝑗−𝑟􀁭􀊅􀁯+𝐶􀁮 2􀈪′ 􀊂𝑖,𝑗,𝑘􀊅􀊂𝜃𝑖𝑗𝑘−𝜃􀁭􀊅􀁯,(3.1) where the primed sums run over nearest neighbours, 𝑟􀁭is the equilibrium bond length, given by 􀁰 􀁱𝑎􀁭, where 𝑎􀁭is the lattice constant, 𝜃𝑖𝑗𝑘 is the angle between the 􀊂𝑖,𝑗􀊅and 􀊂𝑗,𝑘􀊅bonds, and 𝜃􀁭is the equilibrium bond angle (109.471∘for zinc-blende structures). Therefore, it has only two adjustable parameters, the force constants 𝐶􀁭and 𝐶􀁮, which were obtained by Mingo and Broido [61] by computing bulk phonon dispersion relations and adjusting them to match the experimental frequencies of the zone centre longitudinal optical mode, 𝜔𝐿𝑂(𝛤), and the zone edge transverse acoustic mode, 𝜔𝑇𝐴(𝑋). The values so obtained were used in this work, and are reproduced in Table 3.1. The potential proposed by Hammerschmidt et al. [110] for GaAs and InAs surfaces and nanostructures is a carefully parameterised Abell-Tersoff potential [114–117]. The values of its many adjustable parameters for GaAs and InAs were fitted by Hammerschmidt et al. [110] to a large set of reference data that included both experimental and density-functional results for structural and elastic properties of bulk Ga, As, In, GaAs and InAs, and structural and energetic properties of several reconstructed low-index GaAs and InAs surfaces, and are included in Table 3.2. This potential has the functional form 44 3.3. Calculation of the phonon density of states 𝑉=􀈪 𝑖􀈪 𝑗≠𝑖 𝑓(𝐶) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅􀉼𝑉(𝑅) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅−𝑉(𝐴) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅􀉿(3.2a) 𝑉(𝑅) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅=𝐷𝑖𝑗 𝑆𝑖𝑗−1𝑒𝑥𝑝􀉽−𝛽𝑖𝑗􀇽2𝑆𝑖𝑗􀊂𝑟𝑖𝑗−𝑅(􀁭) 𝑖𝑗 􀊅􀊀(3.2b) 𝑉(𝐴) 𝑖𝑗 􀊂𝑟𝑖𝑗􀊅=𝑆𝑖𝑗𝐷𝑖𝑗 𝑆𝑖𝑗−1𝑒𝑥𝑝⎡⎢⎢⎣−𝛽𝑖𝑗􀇿2 𝑆𝑖𝑗 􀊂𝑟𝑖𝑗−𝑅(􀁭) 𝑖𝑗 􀊅⎤⎥⎥⎦(3.2c) 𝐵𝑖𝑗􀊂𝑟𝑖𝑗􀊅=􀊉1+􀉼𝛾𝑖𝑗𝜒𝑖𝑗􀊂𝑟𝑖𝑗􀊅􀉿𝜂𝑖𝑗􀊌−􀁸 􀁹𝜂𝑖𝑗 (3.2d) 𝜒𝑖𝑗􀊂𝑟𝑖𝑗􀊅=􀈪 𝑘∉􀊈𝑖,𝑗􀊋𝑓(𝐶) 𝑖𝑘 (𝑟𝑖𝑘)𝑔𝑖𝑘􀊂𝜃𝑖𝑗𝑘􀊅𝑒𝑥𝑝􀊉􀉼𝛼𝑖𝑘􀊂𝑟𝑖𝑗−𝑟𝑖𝑘􀊅􀉿𝑚𝑖𝑘􀊌(3.2e) 𝑔𝑖𝑘􀊂𝜃𝑖𝑗𝑘􀊅=𝛿𝑖𝑘⎡⎢⎢⎣1+𝑐􀁯 𝑖𝑘 𝑑􀁯 𝑖𝑘 −𝑐􀁯 𝑖𝑘 𝑑􀁯 𝑖𝑘+􀊂ℎ𝑖𝑘−𝑐𝑜𝑠𝜃𝑖𝑗𝑘􀊅􀁯⎤⎥⎥⎦(3.2f) 𝑓(𝐶) 𝑖𝑗 =⎧⎪⎪⎪⎪⎨⎪⎪⎪⎪⎩ 1, 𝑟𝑖𝑗−𝑅(𝐶) 𝑖𝑗 ≤−𝐷(𝐶) 𝑖𝑗 􀁮 􀁯􀉾1−𝑠𝑖𝑛􀊄𝜋𝑟𝑖𝑗−𝑅(𝐶) 𝑖𝑗 􀁯𝐷(𝐶) 𝑖𝑗 􀊇􀊁,􀉥𝑟𝑖𝑗−𝑅(𝐶) 𝑖𝑗 􀉥<𝐷(𝐶) 𝑖𝑗 0, 𝑟𝑖𝑗−𝑅(𝐶) 𝑖𝑗 ≥𝐷(𝐶) 𝑖𝑗 .(3.2g) In all MD calculations presented here, the forces on individual atoms were obtained from the analytical derivatives of the appropriate equations for the total energy of the system. 3.3. Calculation of the phonon density of states Themethodusedtoestimatethephonondensityof states(DOS)inChapter 2is basedontheFouriertransformofthevelocityautocorrelationfunctionand, while it has the advantage of being easy to implement as a post-processing step after MD simulations, provides imprecise results due to factors such as the influence of temperature. In this chapter, to get a more detailed picture and to be able to compare different potentials, a more direct method will be used, based on lattice dynamics. The notation introduced here will also be useful for later chapters. It is well-known that a field defined on the nodes of a crystalline structure periodic along the 𝑂𝑍direction can — as long as it meets certain integrability criteria — be decomposed in terms of harmonic functions of a well-defined 45 3. Influence of the potential on MD thermal conductivity Table 3.2 Parametersof the Hammerschmidtpotential, obtained fromRef. 110. Ga-Ga As-As In-In Ga-As In-As 𝑅𝑖𝑗 􀊂A􀊅2.2625 1.9018 2.6639 2.33824 2.5492 𝐷𝑖𝑗 (eV)1.4159 7.9717 1.5052 1.9561 1.8900 𝛽𝑖𝑗 􀊂A−􀁮􀊅0.9079 1.2165 1.1847 1.5396 1.4549 𝑆𝑖𝑗 1.0646 2.3439 1.2440 1.1543 1.8578 𝛾𝑖𝑗 1.4401 4.8650 4.0976 0.2992 2.2113 𝛼𝑖𝑗 􀊂A−􀁮􀊅0.7469 2.5408 1.2117 −1.3824 1.1816 𝛿𝑖𝑗 0.0050 0.3609 0.0109 0.0424 0.0190 𝑐𝑖𝑗 1.4897 0.1749 1.0853 1.7796 3.9707 𝑑𝑖𝑗 0.8376 0.2140 0.9465 0.6450 0.9486 ℎ𝑖𝑗 −0.3373 −0.1261 −0.4652 −0.4060 −0.5102 𝜂𝑖𝑗 1.0 1.0 1.0 1.0 1.0 𝑚𝑖𝑗 1.0 1.0 1.0 1.0 1.0 𝑅(𝐶) 𝑖𝑗 􀊂A􀊅2.95 3.1 3.5 3.1 3.7 𝐷(𝐶) 𝑖𝑗 􀊂A􀊅0.15 0.1 0.1 0.2 0.1 periodicity indicated by their wave number 𝑘(𝑧). The set of all possible values of 𝑘(𝑧)is called reciprocal space, and it can be generated by periodic translation of a unit cell with length 2𝜋/𝑙𝑧, where 𝑙𝑧denotes the length of the real-space unit cell. A particularly interesting case is that where the field under study representsthedisplacementof each atomin the systemwithrespecttoitsequilibrium position, a minimum of the potential energy which will be arbitrarily taken as 𝑉=0. In a neighbourhood of this point, 𝑉admits a second-order Taylor expansion without zeroth- or first-order terms. Let each unit cell have 𝐵atoms, and 𝑢􀊂𝜇􀊅 𝐼,𝑗 be the displacement in the 𝜇direction of atom 𝑗∈{1,…,𝐵}in unit cell 𝐼with position 𝑙𝑧𝐼. The change in potential energy with respect to the minimum induced by a periodic displacement, 𝑢􀊂𝜇􀊅 𝐼,𝑗 =ℜ􀊊𝑢􀊂𝜇􀊅 􀁭,𝑗 𝑒−𝑖𝑘(𝑧)𝑙𝑧𝐼􀊍, of wave number 𝑘(𝑧), is 𝑉=12􀈪 𝐼,𝐼′ 𝜇,𝜇′,𝑗,𝑗′ 𝜕􀁯𝑉 𝜕𝑢􀊂𝜇􀊅 𝐼,𝑗 𝜕𝑢􀊂𝜇′􀊅 𝐼′,𝑗′𝑢􀊂𝜇􀊅 𝐼,𝑗 𝑢􀊂𝜇′􀊅 𝐼′,𝑗′,(3.3) 46 3.3. Calculation of the phonon density of states or, in terms of complex amplitudes, 𝑉=14ℜ⎧⎪⎪⎪⎨⎪⎪⎪⎩􀈪 𝐼,𝐼′ 𝜇,𝜇′,𝑗,𝑗′ 𝜕􀁯𝑉 𝜕𝑢􀊂𝜇􀊅 𝐼,𝑗 𝜕𝑢􀊂𝜇′􀊅 𝐼′,𝑗′􀊊𝑢􀊂𝜇􀊅 􀁭,𝑗 𝑢􀊂𝜇′􀊅 􀁭,𝑗′𝑒−𝑖𝑘(𝑧)𝑙𝑧[𝐼+𝐼′]+𝑢􀊂𝜇􀊅 􀁭,𝑗 􀉾𝑢􀊂𝜇′􀊅 􀁭,𝑗′􀊁∗𝑒−𝑖𝑘(𝑧)𝑙𝑧[𝐼−𝐼′]􀊍⎫⎪⎪⎪⎬⎪⎪⎪⎭= =14ℜ⎧⎪⎪⎪⎨⎪⎪⎪⎩􀈪 𝐼,𝐼′ 𝜇,𝜇′,𝑗,𝑗′𝑢􀊂𝜇􀊅 􀁭,𝑗 𝑢􀊂𝜇′􀊅 􀁭,𝑗′⎧⎪⎪⎨⎪⎪⎩􀈪 𝐼,𝐼′𝜕􀁯𝑉 𝜕𝑢􀊂𝜇􀊅 𝐼,𝑗 𝜕𝑢􀊂𝜇′􀊅 𝐼′,𝑗′𝑒−𝑖𝑘(𝑧)𝑙𝑧[𝐼+𝐼′]⎫⎪⎪⎬⎪⎪⎭⎫⎪⎪⎪⎬⎪⎪⎪⎭+ +14ℜ⎧⎪⎪⎪⎨⎪⎪⎪⎩􀈪 𝐼,𝐼′ 𝜇,𝜇′,𝑗,𝑗′𝑢􀊂𝜇􀊅 􀁭,𝑗 􀉾𝑢􀊂𝜇′􀊅 􀁭,𝑗′􀊁∗⎧⎪⎪⎨⎪⎪⎩􀈪 𝐼,𝐼′𝜕􀁯𝑉 𝜕𝑢􀊂𝜇􀊅 𝐼,𝑗 𝜕𝑢􀊂𝜇′􀊅 𝐼′,𝑗′𝑒−𝑖𝑘(𝑧)𝑙𝑧[𝐼−𝐼′]⎫⎪⎪⎬⎪⎪⎭⎫⎪⎪⎪⎬⎪⎪⎪⎭. (3.4) Of the two terms in the right-hand side, the first one is not invariant under a translation (𝐼,𝐼′)⟶(𝐼+𝛥,𝐼′+𝛥),𝛥∈ℤ, so it must be zero, while the second one is a sum containing the complex conjugate of each of its terms, therefore making the real-part operator unnecessary. The Hessian matrix of the potential is often called the force-constant matrix, and each of the second derivatives of the potential it comprises will be denoted by 𝐾􀊂𝜇,𝜇′􀊅 𝐼,𝐼′,𝑗,𝑗′. The system’s periodicity implies that force constants can only depend on 𝐼and 𝐼′through 𝐼−𝐼′. Hence, the double sum between curly brackets in Eq. (3.4) can be reduced to the value of its term for 𝐼′=0times the number of unit cells in the system. If the appropriate normalisation factor is now supposed to be included in 𝑢􀊂𝜇􀊅 􀁭,𝑗 and 𝑢􀊂𝜇′􀊅 􀁭,𝑗′,𝑉=12􀈪 𝜇,𝜇′,𝑗,𝑗′𝑢􀊂𝜇􀊅 𝑗􀉾𝑢􀊂𝜇′􀊅 𝑗′􀊁∗􀊊􀈪 𝐼𝐾􀊂𝜇,𝜇′􀊅 𝐼,𝑗,𝑗′𝑒−𝑖𝑘(𝑧)𝑙𝑧𝐼􀊍.(3.5) Here, all the references to the central cell 0have been omitted for brevity. This expression allows a calculation of the normal vibration modes of the infinite lattice to be performed in terms of a finite number of degrees of freedom, those of a single unit cell. Using this quadratic form of the potential in Newton’s second law 𝑚𝑗𝑑􀁯𝑢􀊂𝜇􀊅 𝑗/𝑑𝑡􀁯=−𝜕𝑉/𝜕𝑢􀊂𝜇􀊅 𝑗, a set of linear differential equations is obtained, whose general solution can be expressed in terms of a basis of ex- 47 3. Influence of the potential on MD thermal conductivity 89. Swope, W. C., Andersen, H. C. & amd K. R. Wilson, P. H. B. J. Chem. Phys. 76, 637 (1982). 99. Zhou, X. W., Aubry, S., Jones, R. E., Greenstein, A. & Schelling, P. K. Phys. Rev. B 79, 115201 (2009). 108. Mingo, N. Appl. Phys. Lett. 88, 149902 (2006). 109. Mingo, N. Appl. Phys. Lett. 85, 5986 (2004). 110. Hammerschmidt, T., Kratzer, P. & Scheffler, M. Phys. Rev. B 77, 235303 (2008). 111. Thomas, J. A., Intzi, R. M. & McGaughey, A. J. H. Phys. Rev. B 81, 045413 (2010). 112. Sellan, D. P., Landry, E. S., Turney, J. E., McGaughey, A. J. H. & Amon, C. H. Phys. Rev. B 81, 214305 (2010). 113. Yang, X., To, A. C. & Tian, R. Nanotechnology 21, 155704 (2010). 114. Tersoff, J. Phys. Rev. Lett. 56, 632 (1986). 115. Tersoff, J. Phys. Rev. B 37, 6991 (1988). 116. Tersoff, J. Phys. Rev. B 38, 9902 (1988). 117. Tersoff, J. Phys. Rev. B 39, 5566 (1989). 118. Both, W., Gottschalch, V. & Wagner, G. Crysr. Res. Technol. 21, K85 (1986). 119. Properties of Gallium Arsenide 3rd (eds Brozel, M. R. & Stillman, G. E.) (INSPEC, London, 1996). 120. Steigmeier, E. F. & Kudman, I. Phys. Rev. 132, 508 (1963). 121. Fritsch, J., Pavone, P. & Schröder, U. Phys. Rev. B 52, 11326 (1995). 122. Borcherds, P. H., Alfrey, G. F., Saunderson, D. H. & Woods, A. D. B. J. Phys. C 8, 2022 (1975). 123. Mooradian, A. & Wright, G. B. Solid State Commun. 4, 431 (1966). 124. Semiconductors: Physics of Group IV and III-IV Compounds (ed Madelung, O.) (Springer-Verlag, Berlin, 1982). 125. Semiconductors: Intrinsic Properties of Group IV Elements and III-V, II-VI, and I-VII Compounds (ed Madelung, O.) (Springer-Verlag, Berlin, 1987). 126. Persson, A. I., Koh, Y. K., Cahill, D. G., Samuelson, L. & Linke, H. Nano Lett. 9, 4484 (2009). 54 References 127. Mavrokefalos, A., Pettes, M. T., Saha, S., Zhou, F. & Shi, L. 25th International Conference on Thermoelectrics, 234 (2006). 55 4Surface roughness and thermal conductivity of Si nanowires For it is possible long study may increase and confirm erroneous sentences: and where men build on false grounds, the more they build, the greater is the ruin. Leviathan Thomas Hobbes 4.1. Introduction MD provides a set of useful and easily implementable methods for thermal conductivity calculations but, as seen in Chapters 2 and 3, it also has some important shortcomings. In particular, its purely classical nature limits its applicability to relatively high temperatures, and the fact that it does not treat phonons as first-class objects makes the results from MD calculations somewhat opaque. Moreover, the results are very dependent on the choice of potential. Thus, in order to understand thermal transport in nanowires in further detail, it is desirable to use methods with their roots in more fundamental physics. That is the purpose of the work contained in this chapter. 57 4. Surface roughness and thermal conductivity of Si nanowires The solution of Eq. (3.6a) for a crystalline system with one-dimensional periodicity consists not only of a set of eigenfrequencies 􀊈𝜔♢􀊋, but also of a basis of eigenstates 􀊊𝑤􀊂𝜇􀊅 ♢,𝑗􀊍. This basis will be assumed to be orthogonal, something which is always possible through an appropriate choice of degenerate eigenvectors. It is straightforward to check that, in the related basis 􀊊𝑢􀊂𝜇􀊅 ♢,𝑗 =𝑤􀊂𝜇􀊅 ♢,𝑗/√𝑚𝑗􀊍and its periodic repetitions, the quadratic approximation to the potential energy expressed in Eq. (3.5) becomes diagonal. Hence, for each value of 𝑘(𝑧)the hamiltonian of the system adopts the form of a sum of independent harmonic oscillators, which can be quantised to give 𝑯􀊂𝑘(𝑧)􀊅=􀈪 ♢ℏ𝜔♢􀉾􀊄𝓪† ♢𝓪♢+12􀊇􀊁.(4.1) Here, 𝓪† ♢and 𝓪♢are the ladder operators corresponding to one of the oscillation modes, but can also be interpreted, in the second quantization formalism, as phonon creation and annihilation operators. Each phonon of frequency 𝜔♢ carries an energy ℏ𝜔♢and a linear momentum ℏ𝑘(𝑧)proportional to its wave number. From a statistical point of view, phonons are bosons and thus follow Bose-Einstein statistics: at equilibrium, the average occupation number of a state is 𝑓𝐵𝐸􀊂𝑇;𝑘(𝑧),♢􀊅=1 𝑒ℏ𝜔♢􀊃𝑘(𝑧)􀊆 𝑘𝐵𝑇−1.(4.2) Transport theory is mainly concerned with states slightly out of equilibrium. The methods used to study them for this work will be explained briefly in the following sections. Of particular relevance for understanding the size dependence of thermal conductivity is the role of the boundary, which becomes increasingly more important asthe surface-to-volume ratio increases, andthe orderedor disordered regions therein. For a sufficiently wide nanowire, scattering of phonons by a boundary surface can be approximated by the Casimir formula for bulk systems [128], which predicts a mean free path (MFP) equal to the diameter of the wire times a factor of order unity which depends on the cross-sectional shape. When this source of scattering becomes so dominant as to make any other negligible, something to be expected in very thin crystalline nanowires, it should result in a thermal conductivity proportional to the diameter. This paramet- 58 4.2. Quasi-ballistic transport erisationhasbeenshowntoaffordareasonably good agreementwith theavailable experimental and computational data in this range of widths [129]. On the other hand, experimental data for the lattice thermal conductivity of rough Si nanowires with diameters below 50nm, reported by Hochbaum et al. [130] in 2008, showed values close to the amorphous limit for silicon, which could not be explained by existing theories. Martin et al. [131] put forward a theoretical approach which can fit the experimental results and whose key ingredients are a continuum model, the relaxation time approximation, Fermi’s golden rule (from first order perturbation theory), a Gaussian approximation [132] to the power spectrum of surface roughness with an adjustable parameter and semiempirical parameterisations of the different scattering sources (phononphonon interactions, impurities and the boundary) [36, 133, 134]. Boundary and roughness scattering are thus treated in two different ways (the Casimir formula and perturbation theory, respectively) and then added together under an assumption of statistical independence (a procedure known as Matthiessen’s rule). Since the Casimir formula, as it will be explained later in this chapter, already assumes a disordered boundary so that the probability of a phonon being scattered in a particular direction is independent of its direction of incidence, such double counting of the effect of the boundary on phonons seems unwarranted. Moreover, due to the number of adjustable parameters and unassessed approximations present in that description, it is of little predictive value. In order to contribute to the solution of this controversy, Si was chosen as the material for the nanowires studied in this chapter, in which the results a completely atomisticcalculation of boundary scattering in verythinnanowires is presented. The system under study was an hexagonal monocrystalline Si nanowire oriented along the [111]direction, structurally identical to the InAs, InP and GaAs nanowires studied previously except for the fact that all its atoms belong to the same element. 4.2. Quasi-ballistic transport Consider two heat baths at temperatures 𝑇+𝛥𝑇/2and 𝑇−𝛥𝑇/2joined by a quasi-one-dimensional structure — such as a nanowire — of length 𝐿and cross-sectional area 𝐴. Such a setup is depicted schematically in Fig. 4.1. Each bath is large enough to be considered at equilibrium in spite of the heat flowing across the scattering region. Therefore, the occupation number of a level 59 4. Surface roughness and thermal conductivity of Si nanowires Figure 4.1 Scheme of a nanowire inserted between two heat baths. T+ΔT/2 T-ΔT/2 Scattering region L at the thermostats can be evaluated using Eq. (4.2) at the appropriate temperature. If there is a probability 𝑝𝑡𝑟𝑎𝑛𝑠􀊂𝑘(𝑧),♢􀊅that a phonon of wave number 𝑘(𝑧) and frequency 𝜔♢􀊂𝑘(𝑧)􀊅be transferred between the two ends of the scattering region, the total heat current must be calculated as a balance between the energy transferred left-to-right and right-to-left by phonons per unit time and area 𝑗(𝑧) 𝑄=1𝐴􀈪 ♢ 𝜋 𝑙𝑧 􀈧 􀁭􀉾𝑓𝐵𝐸􀊄𝑇+𝛥𝑇 2;𝑘(𝑧),♢􀊇− 𝑓𝐵𝐸􀊄𝑇−𝛥𝑇 2;−𝑘(𝑧),♢􀊇􀊁ℏ𝜔♢𝑝𝑡𝑟𝑎𝑛𝑠􀊂𝑘(𝑧),♢􀊅𝑣(𝑧) 𝑔,♢ 𝐿𝑑𝑘(𝑧) 2𝜋/𝐿.(4.3) Provided that 𝛥𝑇≪𝑇, the difference between equilibrium distributions in the integrand can be approximated by its first-order Taylor expansion, and the whole equation rewritten as 𝑗(𝑧) 𝑄=𝛥𝑇 𝐴􀈧𝜕𝑓𝐵𝐸 𝜕𝑇ℎ𝜔𝒯(𝜔)𝑑𝜔 2𝜋,(4.4) where 𝒯(𝜔)is known as the transmission function — or simply the transmission — of the nanowire at frequency 𝜔, and the integral over frequencies can be understood to run either from 0to ∞, with 𝒯(𝜔)=0for values of 𝜔beyond the upper edge of the vibrational spectrum (𝜔𝑈) or from 0to that limit. From Eq. (4.3), it is clear that 0≤𝒯(𝜔)≤𝒩(𝜔), where 𝒩(𝜔)is the number of vibrational modes with frequency 𝜔. The upper limit can only be reached if all the 60 4.3. Transmission calculations transmission probabilities are 1,i.e., if there is no scattering at all in the central region. Since the average temperature gradient across the nanowire is −𝛥𝑇/𝐿, a combination of Eq. (4.4) and Fourier’s law (2.1) yields a thermal conductivity 𝜅= 𝑗(𝑧) 𝑄 (𝛥𝑇/𝐿)=𝐿 2𝜋𝐴􀈧𝜕𝑓𝐵𝐸 𝜕𝑇ℎ𝜔𝒯(𝜔)𝑑𝜔. (4.5) In macroscopic problems, 𝜅is independent from 𝐿. However, Eq. (4.5) implies that this is not always the case in the nanoscale. In particular, if there is no scattering, 𝒯(𝜔)=𝒩(𝜔)∀𝜔∈[0,𝜔𝑈], and it is the thermal conductance, 𝐺𝑇≔𝐴𝑗(𝑧) 𝑄 𝛥𝑇 =𝐴𝐿𝜅, (4.6) instead of the thermal conductivity, that is independent of the length of the nanowire. This regime of thermal transport is known as ballistic (or, more precisely, quasi-ballistic when the transmission is not perfect) as opposed to the more usual one, referred to as ohmic due to its resemblance to Ohm’s law for electric resistors. Thus, in the ballistic regime, thermal conductivity is not a especially useful concept. It is unrealistic to expect the ballistic regime to be valid for long nanowires, but Eq. (4.5) can still be useful in an ohmic setting if a suitable transmission is defined. The problem of characterising boundary scattering in thin nanowires will be approached in two steps in the following two sections. First, a method for calculating a detailed form of the phononic transmission across a localised defect that can be treated in the ballistic regime (its length being small enough that phonons remain coherent, in quantum terms) will be presented, and then it will be used to calculate the scattering cross-section of the localised defect, which in turn can yield a transmission valid in the ohmic regime. 4.3. Transmission calculations For a periodic system, diagonalising 𝑫is equivalent to diagonalising 𝑲: their eigenvalues coincide and their eigenvectors are trivially related. If the system under consideration is of a more general nature, periodic or aperiodic, finite or infinite, the convenience of always working with a finite number of elements [using Eq. (3.6a)] has to be abandoned and the normal modes of the 61 4. Surface roughness and thermal conductivity of Si nanowires system obtained by solving the general equation 𝑲|𝑘⟩=𝜔􀁯|𝑘⟩or, in a homogeneous form, 􀊂𝜔􀁯𝟏−𝑲􀊅|𝑘⟩=𝟎. (4.7) An inhomogeneous version of this equation, with a non-zero matrix in the right-hand side, can be solved using the fundamental solution (or resolvent) 􀊂𝜔􀁯𝟏−𝑲􀊅−􀁮. In the context of thermal transport studies, this is known as the phononicGreen’sfunction forhistoricreasons. Thereare well-knownmethods to calculate quasi-ballistic transmissions in the harmonic approximation using Green’s functions [16], but for the work presented here a new algorithm was developed which provides more detailed information in the form of transition probabilities between the individual vibrational modes in the left and the right part of the scattering region. Let us consider a perfectly crystalline nanowire formed by repetition of a (possibly non-primitive) unit cell of length 𝑙𝑧chosen so that, as in Chapter 3 and owing to the limited range of the potential, a given unit cell only interacts with its first neighbours. Its stiffness matrix will be denoted by 𝓚, of which the only different non-zero building blocks are 𝓚􀁭and 𝓚􀁮, which describe the harmonic interactions between an unit cell and itself and between an unit cell and the one to its right, respectively. For each 𝑘(𝑧), the eigenvalues of the dynamical matrix are the allowed frequencies of the system squared, and the corresponding eigenvectors are the wave functions which describe the movements of each atom in the unit cell when the system is oscillating in a particular mode. Alternatively, it ispossible toobtain the allowed values of𝑘(𝑧)fora given 𝜔by solving the generalised eigenvalue problem: ⎛⎜⎜⎝𝜔􀁯𝟏−𝓚􀁮−𝓚† 􀁮 𝟏 𝟎 ⎞⎟⎟⎠𝑐=𝜆⎛⎜⎜⎝𝓚􀁮𝟎 𝟎 𝟏⎞⎟⎟⎠𝑐. (4.8) Obviously, the eigenvectors 𝑐thus obtained are defined over two unit cells. It can be easily checked that the unitary eigenvalues of the problem are 𝑒𝑖𝑘(𝑧)𝑙𝑧 and that the first half of each 𝑐is the corresponding 𝑤, an eigenvector of the dynamical matrix. In the remainder of this section, 􀊉􀉥𝑘(𝑧) ♢􀈋􀊌will denote the set of normal modes of the perfect system for a particular 𝜔, as defined over the whole nanowire, with wave numbers 􀊈𝑘(𝑧) ♢􀊋. Although the system is infinite, for normalisationpurposesavery largenumber 𝑁𝑧of unit cells will be considered, 62 4.3. Transmission calculations keeping in mind that the final expressions will be valid in the limit 𝑁𝑧⟶∞; therefore, 􀈘𝑘(𝑧) ♢􀉥𝑘(𝑧) ♣􀈋=𝑁𝑧𝛿♢♣. This implies that 􀉼𝑤♢(𝐼)􀉿∗⋅𝑤♣(𝐼)=𝛿♢♣, if 𝑤♢(𝐼)is the restriction of 􀉥𝑘(𝑧) ♢􀈋to the 𝐼-th unit cell. For notational brevity, 𝑤♢(0)will be simply denoted as 𝑏♢. In 𝑘(𝑧)-space, the Green’s function of this perfect nanowire can be expressed as [16]: 𝒈+􀊂𝜔,𝑘(𝑧)􀊅=1 𝑁𝑧􀈪 ♢􀉥𝑘(𝑧) ♢􀈋􀈘𝑘(𝑧) ♢􀉥 𝜔􀁯−𝜔􀁯 ♢+𝑖𝜂,(4.9) for 𝜂⟶0+. Strictly speaking, this is the causal Green’s function. The anticausal Green’s function 𝒈−would be obtained if 𝜂⟶0−was taken instead. A defect can be introduced in the nanowire by replacing the unit cell 𝐼=0 of the perfect system with a different set of atoms. This operation breaks the translationalsymmetry ofthe system, whichbecomes aperiodic. If the stiffness matrix of the defective nanowire is represented by 𝑲, the impurity operator, 𝑽, is defined as 𝑽≔𝑲−𝓚, (4.10) and the 𝑡-matrix which connects both situations, as 𝒕+=𝑽􀊂𝟏−𝒈+𝑽􀊅−􀁮 =􀊂𝟏−𝑽𝒈+􀊅−􀁮𝑽. (4.11) Provided that 𝑙𝑧is large enough, the real-space representations of these two operators are nonzero only over the unit cell 𝐼=0, that is, if 𝒕+(𝐼,𝐼′)is the submatrix of 𝒕+connecting cells 𝐼and 𝐼′, only 𝒕+(0,0)is non-zero, and the same applies to 𝑽. The normal modes of the system containing the defect, at each frequency 𝜔, will be denoted by 􀊈􀉤𝑞♢􀈊􀊋, and their restrictions to the central unit cell (𝐼=0) by 􀊈𝑒♢􀊋. They are related to 􀊈􀉤𝑘♢􀈊􀊋, since Eq. (4.7) for the defective nanowire can be recast in the inhomogeneous form 􀊂𝜔􀁯𝟏−𝓚􀊅􀉤𝑞􀈊=𝑽􀉤𝑞􀈊(4.12) and solved using its fundamental solution, which is precisely 𝒈+. This process leads to the Lippmann-Schwinger equation 63 4. Surface roughness and thermal conductivity of Si nanowires 4.5. The Casimir mean free path In 1938, H. Casimir theoretically derived the MFP for particle-like carriers in thin wires under diffuse boundary conditions [128]. The Casimir formula is valid under the assumption that phonons behave like classical point-like particles bouncing off the walls of a translationally-symmetric wire with rough boundaries in such a way that after each collision phonons are isotropically re-emitted at random and lose any memory of their incident direction. In this setup, the length of the wire and the wavelengths of phonons do not enter the problem; therefore, the phononMFP mustbe proportional to 𝑑, the only length scale left. In fact, it can be proven by simple geometrical arguments that 𝛬Casimir =3𝜋 4⟨𝐷⟩,(4.36) where ⟨𝐷⟩is the average distance from a random point inside the wire to a random point at its boundary with the same value of 𝑧, understood as a double average over the cross-sectional area and over the corresponding boundary curve. When a constant-𝑧slice of the nanowire is a regular polygon, whose sides are segments of straight lines, 𝛬Casimir is particularly easy to calculate semi-numerically. In that case, the average distance from a point to the whole boundary is equal to its average distance to a particular side of the polygon, due to rotational symmetry. Thus, the integral over the boundary can be performed analytically as a simple integral over a segment. The Casimir MFP for regular polygons of up to 20sides is shown in Fig. 4.2. It can be seen that 𝛬Casimir converges rapidly to 𝑑as the number of sides is increased; indeed, 𝛬Casimir =𝑑is the analytic result for a cylindrical nanowire. Of particular interest for this work is the case of an hexagonal prism, for which the Casimir MFP is 0.907𝑑. This approach was extended by Ziman [137] to consider the effect of partly specular surfaces, yielding a correction factor 􀁮+𝑝 􀁮−𝑝, where 𝑝is the coefficient of specularity, ranging from 0for diffusive scattering to 1for mirror-like reflection. Work by Dingle [137, 138] showed that when some intrinsic bulk scattering mechanism acts together with boundary scattering, the exact solution of the BTE yields nearly the same conductivity as if one used an effective MFP given by Mathiessen’s approximated rule, 𝛬−􀁮 ≃𝛬−􀁮 intrinsic +𝛬−􀁮 Casimir. For thin wires the boundary term dominates, and thus Casimir’s diffuse boundary MFP determines a lower bound for the thermal conductivity. However Casimir’s deduction neglects factors such as the atomistic structure of the 70 4.6. The Stillinger-Weber potential Figure 4.2 Casimir MFP for nanowires of regular polygonal cross-section (3to 20sides) as a fraction of their outer diameter. The solid line is provided only as a guide to the eye. d 3 6 9 12 15 18 number of sides 0.5 0.6 0.7 0.8 0.9 1.0 1.1 ΛCasimir / d boundary and the wave nature of phonons, which could come into play for very small diameters. It is therefore desirable to check its validity using atomistic approaches. 4.6. The Stillinger-Weber potential In this work, interactions between the atoms in the system were described by means of the well-known Stillinger-Weber (SW) potential. This model has been used to describe the crystalline and liquid phases of bulk Si [43], and more recently to investigate the structures, nanomechanics, phonon spectra and thermal conductivities of thin Si nanowires (see, e.g., Refs. 41, 139 and those cited therein). It is a potential with two- and three-body contributions in the general form of Eq. (2.3) and with the following functional choices [43]: 71 4. Surface roughness and thermal conductivity of Si nanowires Table 4.1 Parameters of the SW potential for Si, from Ref. 43. 𝜎=0.2091nm 𝜖=2.1678eV 𝐴=7.049556277 𝐵=0.6022245584 𝑎=1.80 𝜆=21.0 𝑝=4 𝑞=0 𝛾=1.20 𝑉(􀁯) 𝑖𝑗 (𝑟)=𝜖𝑓(􀁯)􀊃𝑟𝜎􀊆(4.37a) 𝑉(􀁰) 𝑖𝑗𝑘 􀊂𝑟𝑖,𝑟𝑗,𝑟𝑘􀊅=𝜖𝑓(􀁰)􀊄𝑟𝑖 𝜎,𝑟𝑗 𝜎,𝑟𝑘 𝜎􀊇(4.37b) 𝑓(􀁯)(𝑟)=⎧⎪⎪⎨⎪⎪⎩𝐴(𝐵𝑟−𝑝−𝑟−𝑞)𝑒𝑥𝑝􀊈(𝑟−𝑎)−􀁮􀊋, 𝑟<𝑎 0, 𝑟>𝑎 (4.37c) 𝑓(􀁰)􀊂𝑟𝑖,𝑟𝑗,𝑟𝑘􀊅=ℎ􀊂𝑟𝑖𝑗,𝑟𝑖𝑘,𝜃𝑖𝑗𝑘􀊅+ℎ􀊂𝑟𝑗𝑖,𝑟𝑗𝑘,𝜃𝑗𝑖𝑘􀊅+ℎ􀊂𝑟𝑘𝑖,𝑟𝑘𝑗,𝜃𝑘𝑖𝑗􀊅(4.37d) ℎ􀊂𝑟𝑖𝑗,𝑟𝑖𝑘,𝜃𝑖𝑗𝑘􀊅=⎧⎪⎪⎨⎪⎪⎩𝜆𝑒𝑥𝑝􀊉𝛾􀊂𝑟𝑖𝑗−𝑎􀊅−􀁮+𝛾(𝑟𝑖𝑘−𝑎)−􀁮􀊌􀊃𝑐𝑜𝑠𝜃𝑖𝑗𝑘+􀁮 􀁰􀊆􀁯, 𝑟𝑖𝑗,𝑟𝑖𝑘 <𝑎 0, otherwise. (4.37e) The optimal parameters for Si were also taken from Stillinger and Weber’s original paper [43], and are included in Table 4.1 4.7. Computational details According to Sections 4.3 and 4.4, the theoretical approach for obtaining the thermal conductivity of a nanowire can be summarised as follows: compute the Green’s function of a perfect nanowire, use it in conjunction with 𝑽 to calculate the scattering cross section of any defect of interest for all possible frequencies andmodes employing Eqs. (4.28) and(4.11), convert this set ofvalues to MFPs and substitute them in Eq. (4.35) in order to obtain the thermal conductivity. Therefore, the crucial missing object is the submatrix 𝒈+(0,0): a block from the diagonal of the real-space representation of the Green’s function of an infinite, perfect nanowire. This can, obviously, be approximated to an arbitrary degree by a block in the central part of the diagonal (i.e., far from the edges) of the real-space representation of the Green’s function of a finite 72 4.7. Computational details but very long nanowire. For this work an extremely efficient method to obtain such blockwas used, decimation[140–142], aniterative renormalisation-group approach which operates with the two non-zero blocks of the interatomic force constant matrix for the perfect nanowire yielding, at its 𝑗-th iteration, 𝒈+(0,0) for a nanowire with 2𝑗copies of the original unit cell, thereby quickly reaching macroscopicdimensions(since𝑙𝑜𝑔􀁯6.022⋅10􀁯􀁰 ≃79). With36decimationsteps, this calculation was fully converged with respect to the number of steps and was insensitive to the precise value of the imaginary part of 𝜔􀁯— the variable denoted as 𝜂in Eq. (4.17) — which was taken as 􀊂10−􀁲 THz􀊅𝜔. All the systems for which force constant matrices were calculated were relaxed to their minimum-energy configurations, but the degree of surface reconstruction afforded by the SW potential is rather limited due to its being optimised for bulk silicon. It must be noted that, in contrast to the MD models of previous chapters, no rigid boundary conditions are needed for the Green’s function calculations undertaken here. Perfect [111]nanowires of hexagonal cross-section have 𝐷􀁰symmetry (like an equilateral triangle): they are invariant under the identity operation 1, under inversions about three axes separated by 2𝜋/3(operations A, B and C), and under 2𝜋/3and 4𝜋/3rotations around 𝑂𝑍(operations D and E). 𝐷􀁰has three irreducible representations (irreps) denoted as 𝛤􀁮,𝛤􀁯and 𝛤􀁰, and a character table like the one in Table 4.2. As a consequence, representations of linear operators such as the interatomic force matrix and the Green’s function of the nanowire can be reduced to a block-diagonal form in a symmetry-adapted basis. Such basis was constructed in two steps. First, the incomplete projection operators [143] associated to the three irreps were found, in the canonical basis formed by the displacements along 𝑂𝑋,𝑂𝑌and 𝑂𝑍of all the atoms in a unit cell. Then, an orthonormal basis was extracted from each of these rankdeficient matrices. The union of the three bases is precisely the symmetryadapted basis. Harnessing symmetries was essential in order to make the whole calculation process feasible, since the complexity of matrix inversion and other related operations is proportional to the cube of the matrix dimensions. Symmetries were used in the calculation of normal modes — the three blocks ofthe dynamicalmatrix can bediagonalised separately, andfor instance vibrational modes that transform like translation under the action of 𝐷􀁰come from the 𝛤􀁰-adapted part of 𝑫— and in the decimation process. However, symmetry is broken by the introduction of defects, and thus the sparse LU decomposition [144] employed to calculate the matrix elements of 𝒕+used in Eq. 73 4. Surface roughness and thermal conductivity of Si nanowires Table 4.2 Character table for group 𝐷􀁰. 1A,B,C D,E 𝛤􀁮1 1 1 𝛤􀁯1 −1 1 𝛤􀁰2 0 −1 (4.28) is, by a large margin, the most time-consuming part of the calculation. The SW potential, its analytical derivatives and the numerical calculation of its Hessian according to Eq. (3.9) where implemented in C using LAPACK built on the highly optimised Goto version of BLAS [145]. The code for the decimation process was ported to C from a Mathematica®notebook kindly provided by Dr. Natalio Mingo. The rest of the code was implemented in Python and run in parallel on 16processors. Each CPU ran the calculations for a set of frequencies; in the harmonic approximation, different frequencies can be treated independently, thereby allowing a linear scaling of performance with number of processors. 4.8. Results and discussion A nanowire with a diameter 𝑑=2.22nmwas considered — four atomic layers in the radial direction, 182 atoms in the unit cell — as the starting perfect system. As in previous chapters, thin nanowires were deemed the most interesting because of their lower similarity to the bulk. Moreover, real-space Green’s function methods are even more limited than MD-based models with regard to the number of atoms that can be treated, because of their different computational complexities (cubic vs. linear scaling with the number of atoms). In order to simulate the effect of surface roughness, two scenarios were investigated: shallow roughness, where only atoms from the outermost layer were removed at random, with 50%probability; and deep roughness, where, on top of the existing shallow roughness, deep semi-spherical cavities were dug along the wire surface. An example of each case, along with an image of the perfect nanowire, is shown in Fig. 4.3. The associated scattering cross sections were then computed using Eq. (4.28), and the MFPs and relaxation times were derived from them. 74 4.8. Results and discussion Figure 4.3 𝑑=2.22nmSi nanowire: perfect (left), with shallow surface roughness (centre) and with deeper surface cavities (right) Figure 4.4 (top) shows the spectrum of the nanowire as obtained from the diagonal form of the dynamical matrix for each value of 𝑘(𝑧). For comparison, the bottom panel of the same figure shows the same calculation performed with other of the most used potentials for Si, the Tersoff potential [116]. This potential was also implemented in C and a subset of the calculations presented here repeated with it, as well as with a parameterisation of the SW potential for germanium [146], with comparable conclusions. Comparing both panels of Fig. 4.4, it canbe seenthatthe SW potentialoverestimates the upperedgeof the vibrational spectrum, a suspicion confirmed by ab initio and experimental results for bulk Si [147]. Fortunately, the high-frequency part of the spectrum has a very small influence on thermal conductivity. The Tersoff potential also has its shortcomings, such as not predicting the diamond structure as the ground state of bulk silicon and inaccuracies in the prediction of bulk elastic constants [148]; this goes to show that, in general, there is no “perfect” semiempirical potential. On the other hand, the fact that the results presented here are robust with respect to the change of potential lends them greater weight. The averagerelaxation times for each frequency are shown in Fig. 4.5. Both the exact results and those obtained using the Born approximation diverge at low frequencies, indicating quasi-ballistic transmission. At higherfrequencies, the exact relaxation times suggest that the Casimir approximation is adequate. There is, however, a striking difference of 1−2orders of magnitude between the red and green curves, with the Born approximation resulting in an unreal- 75 4. Surface roughness and thermal conductivity of Si nanowires Figure 4.4 Vibrational spectrum of a 𝑑=2.22nmnanowire obtained using the SW (top) and Tersoff (bottom) potentials. Line styles correspond to irreps: full⇒𝛤􀁮, dotted⇒𝛤􀁯, dashed⇒𝛤􀁰. 020406080100120140−1.0−0.50.00.51.0()lzkz/π020406080100120 ω (THz) ω (THz) 76 4.8. Results and discussion Figure 4.5 Relaxation times, averaged over all the available modes for each frequency, in a 𝑑=2.22nmwire with half of its outermost atoms removed, calculated using the exact 𝒕+matrix and the Born approximation. The Casimir limit is also plotted for comparison. The shadowed area corresponds to the part of the spectrum for which the resistance of the contacts would be the dominating factor, as explained in the text. istically highestimate of the scatteringcross section. This isa general featureof the approximation in this context and becomes even worse when larger defects are introduced. Further evidence of this failure is the fact that, if the total reflectance of a single defective segment is calculated using Eq. (4.25) and summing over one of the subscripts, and again introducing the perturbative approximation 𝒕+≃ 𝑽, for most frequencies this reflectance is much larger than the transmission of the perfect system. This is a clearly absurd result which, if substituted into Eq. (4.5) and integrated, would yield a negative value for the thermal conductivity. Surface roughness with a characteristic size larger than the size of the simulation cell (1.9nm) is not included in the simulation and thus the scattering of longer-wavelength/lower-frequency phonons is Rayleigh-like, nearly ballistic. The contribution of this part of the spectrum to the thermal conductivity is, however, negligible if the frequency dependence of the transmission probability between the contacts used for measuring the thermal conductance and the 77 4. Surface roughness and thermal conductivity of Si nanowires nanowire itself is taken into account. As shown in Ref. 149, it is proportional to 𝜔􀁯. This probability was included in the thermal conductivity calculation by using a composition rule for the transmission of the wire plus contact system [150]. The region where contact scattering dominates the composition, causing the results from 𝑡-matrix calculations alone to be insufficient, is shown shadowed in Fig. 4.5. Figure 4.6 compares the thermal conductivities calculated from Eq. (4.35) using MFPs predicted by Eq. (4.28) —in red—, the Born approximation — dashed green— and the Casimir formula with the appropriate form factor — dotted blue— for the system discussed in the foregoing paragraph. The exact MFPs afford a thermal conductivity in reasonable agreement with the Casimir approximation, whereas the perturbative result is qualitatively and quantitatively different, reaching saturation at much lower temperature and conductivity. The values shown here agree in order of magnitude with those obtained in Ref. 151 for rough Si nanowires using MD simulations. As mentioned before, there could be some overestimation of the conductivities due to the fact that the SW potential yields phonon frequencies above their true values, but this would affect the three curves in Fig. 4.6 and thus not undermine this conclusion. Since very thin nanowires are those furthest removed from the context of the derivation of the Casimir formula (which is known to be valid for thick ones), these results suggest that such formula should be a good approximation also for all larger thicknesses. The role of the contact-nanowire transmission (less important for thick wires) in suppressing the divergence at low frequencies would be played in that case by the vanishing, bulk-like number of available states for each frequency [36]. It is possible to go well below the Casimir value by blocking the phonons using defects which penetrate deeper into the nanowire. Figure 4.7 shows the effect on the conductivity (computed at 𝑇=1000K) of removing an almost semi-spherical cluster of up to 100atoms from each 1.9nm-long segment of the wire. The conductivity is normalised to the value obtained by the Casimir formula. As before, the Born approximation overestimates the thermal resistance by an order of magnitude. From the 𝑡-matrix results it can be concluded that the reduction in conductivity resulting from further removal of atoms is rather slow once about a quarter of the cross-sectional area of the wire has been removed. Thus, it is difficult to achieve a reduction in conductivity of more than one order of magnitude with respect to the Casimir limit without compromising other desirable properties or even the structural stability of the 78 4.8. Results and discussion Figure 4.6 Thermal conductivity of a 𝑑=2.22nmnanowire with half of its outermost atoms removed, as a function of temperature, calculated using Eq. (4.35) either with the exact 𝑡-matrix, the Born approximation or the Casimir MFP. 0 200 400 600 800 1000 T(K) 0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.5 κW m K Using t+ Using V Casimir system. The progressively smaller efficiency of further removal of atoms is to be expected if the situation is compared, qualitatively, to the scattering of phonons by spherical nanoparticles studied by Kim and Majumdar [152], who suggest the interpolation formula 𝜎−􀁮 =𝜎−􀁮 􀃱􀂎􀂦􀂙􀂒􀂖􀂔􀂕 +𝜎−􀁮 􀂛􀂒􀂎􀂟−􀂔􀂜􀂚􀂒􀂡􀂟􀂖􀂐􀂎􀂙, resulting in a scattering efficiency that increases quickly with the radius of the sphere when it is small, but simply oscillates around the geometrical limit for larger radii. The possibility of reducing wire conductivity below the Casimir limit had been investigated in the past using non-atomistic approaches. The Montecarlo work by Moore et al. [153] introduced deep boundary roughness in the form of sawtooth boundaries. They found that phonon backscattering can cause the coefficients of specularity to become negative, indicating MFPs below the Casimir limit. However, neither their predictions nor the ones reported in this work match the extremely low experimental conductivities found in Ref. 130. This is especially surprising since the depth of the disordered layers in the experimental nanowires is smaller (relative to their diameter) than in the simulations. All of this and the difference in order of magnitude between the exact 79 5. Thermoelectric properties of hybrid organic-inorganic superlattices Figure 5.2 Left: a tri-thiophene molecule, with (top) or without (bottom) a lateral phenyl group, connected to a pair of hydrogen-passivated semiconductor atoms. Right: fragment of a SiGe+tri-thiophene superlattice, showing a monolayer of tri-thiophene molecules inserted between two blocks of a random Si0.5Ge0.5 alloy. question is investigated in this chapter; it is concluded that HOI materials can indeed display very low thermal conductivities and enhanced 𝑍𝑇, and that they can be fine tuned by organic chemistry techniques. It is also found that using a semiconductor alloy as the inorganic component is crucial to obtain a high 𝑍𝑇in the HOI structures. The particular systems investigated here are made of periodically repeated layers of monocrystalline Si, or of a SiGe alloy, separated by self-assembled monolayers (SAM) of tri-thiophene (see Fig. 5.2). It may not be easy to synthesise a HOI superlattice containing SiGe, since the high temperatures typically required to grow the semiconductor may destroy the organic part. Ref. 162 presents various alternative synthesis approaches already used in other systems. For example, it would be possible to roll up an epitaxial layer of SiGe coated with the organic SAM, in the way already demonstrated for other hybrid HOIs in Refs. 165–167. Substrate transfer techniques may also be an option to circumvent this problem. SAMs of related molecules, such as 𝜔-thiophene-functionalised 𝑛-alkyltrichlorosilane, allyl phenyl thiophene ether and thiophene-terminated alkyl chains, have been experimentally grown on Si substrates [176–178]. The choice of SiGe for the present work is based on ease of calculation, but the physical phenomena identified by this study are likely to take place in any generic HOI superlattice that uses a thermoelectric alloy as the inorganic component. From an experimental point of view, it may be simpler to employ other alloys such as BiSbTeSe, which are compatible with low temperature growth and wet chemistry techniques. 86 5.2. Thermoelectric coefficients 5.2. Thermoelectric coefficients Ifanelectricfield𝐸(𝑧)anda temperature gradient𝜕𝑇/𝜕𝑧areappliedtoasystem such as the one in Fig. 5.1 along the 𝑂𝑍direction (horizontal axis in the figure) charge and energy currents will appear. Provided that 􀉤𝐸(𝑧)􀉤and 􀉤𝜕𝑇/𝜕𝑧􀉤 are small enough, those thermal and electric currents will be linearly related to these thermodynamic forces. Although an HOI superlattice is clearly anisotropic, when only forces along the 𝑂𝑍direction are considered the resulting currents (𝑗(𝑧)and 𝑗(𝑧) 𝑄) will be parallel to them because of inversion symmetries with respect to any plane containing the 𝑂𝑍axis. Therefore, the linear transport regime can be described in terms of the following two scalar phenomenological relations: 𝑗(𝑧)=𝑙𝐸𝐸𝐸(𝑧)+𝑙𝐸𝑇􀊄−𝜕𝑇 𝜕𝑧􀊇(5.2a) 𝑗(𝑧) 𝑄 𝑇=𝑙𝑇𝐸𝐸(𝑧)+𝑙𝑇𝑇􀊄−𝜕𝑇 𝜕𝑧􀊇.(5.2b) The left-hand sides have been chosen [179] so as to ensure that the sum of their products by the correspondingthermodynamic forces, 𝑗(𝑧)𝐸(𝑧)+𝑇−􀁮𝑗(𝑧) 𝑄􀊂−𝜕𝑇/𝜕𝑧􀊅, is proportional to a valid entropy source term, thereby allowing Onsager’s reciprocity relations [180] to be used, which in this case means that 𝑙𝐸𝑇 =𝑙𝑇𝐸. It must be noted, however, that Onsager’s results were originally developed for macroscopic systems and that they cannot be simply assumed to be valid in the nanoscale. In the sixties, T. L. Hill solved a related problem, namely the a priori non-applicability of conventional equilibrium thermodynamics to small systems. His approach began by considering a large ensemble of such elements, well in the thermodynamic limit, and using it to develop equations for the average nanosystem. The resulting formalism, known as nanothermodynamics, has been successfully applied to several kinds of systems, including micelles [181] and nanosolids [182]. More importantly for the present chapter, it has recently been extended to non-equilibrium situations [183]. The most important consequence drawn from that theoretical development is that, even though the theoretical reasoning leading to Onsager’s reciprocity relations has to be modified to take into account the non-extensive character of nanothermodynamics, those relations can still be expected to hold. Thus, there is a solid theoretical basis for relying on Onsager’s reciprocity in the context of, e.g., a self-assembled molecular monolayer of the kind treated in this chapter. 87 5. Thermoelectric properties of hybrid organic-inorganic superlattices By considering some particular cases, the four phenomenological coefficients in Eqs. (5.2) can be identified with combinations of more usual physical parameters. As regards the diagonal coefficients, when 𝜕𝑇/𝜕𝑧=0, Eq. (5.2a) is recognisable as a microscopic version of Ohm’s law; thus, 𝑙𝐸𝐸 =𝜎. On the other hand, 𝜅, as used in Fourier’s law (2.1), is defined for 𝑗(𝑧)=0(as opposed to 𝐸(𝑧)=0) so, according to Eqs. (5.2), 𝜅=𝑇􀊂𝑙𝑇𝑇−𝑙􀁯 𝑇𝐸/𝜎􀊅. At this point, only one coefficient remains in its original form, precisely the one coupling electric and thermal transport. The earliest known manifestation of thermoelectric phenomena, first observed in 1821 and published in 1823 [184], is known as the Seebeck effect. In its simplest form, it consists of the fact that if a temperature difference 𝛥𝑇is applied between the ends of a bar built from a metal or a semiconductor, an open-circuit voltage difference 𝛥𝑉can be measured between them. The Seebeck coefficient is then defined as 𝑆=−􀊄𝛥𝑉 𝛥𝑇􀊇𝑗(𝑧)=􀁭 =􀊄𝐸(𝑧) 𝜕𝑇/𝜕𝑧􀊇𝑗(𝑧)=􀁭 =𝑙𝐸𝑇 𝜎.(5.3) As a consequence, Eqs. (5.2) may be rewritten in terms of more experimentally meaningful coefficients as 𝑗(𝑧)= 𝜎𝐸(𝑧)+𝜎𝑆􀊄−𝜕𝑇 𝜕𝑧􀊇(5.4a) 𝑗(𝑧) 𝑄=𝜎𝑆𝑇𝐸(𝑧)+􀊂𝜅+𝜎𝑆􀁯𝑇􀊅􀊄−𝜕𝑇 𝜕𝑧􀊇.(5.4b) It is these coefficients that enter the definition of the thermoelectric figure of merit 𝑍, introduced in the previous section: 𝑍=𝜎𝑆􀁯 𝜅.(5.5) The numerator of this expression is known as the power factor of the material, 𝑃. Disregarding electron-phonon interactions, 𝑃depends mainly on the electronic band structure of the material under study. On the other hand, it has already been mentioned that in semiconductors 𝜅has two contributions, 𝜅𝑙due to phonons and 𝜅𝑒associated to electrons, and that the first dominates. Therefore, an ideal thermoelectric material would behave like a crystal (with high conductivity) for electrons but like a glass (with very low conductivity) for phonons [185]. 88 5.2. Thermoelectric coefficients Even thoughthesuperlattices underconsiderationdonotpossesscomplete translational symmetry in the 𝑂𝑋and 𝑂𝑌directions, with regard to heat and charge carrier distributions, mesoscopic volume elements may be considered that contain a large enough number of molecules that their properties only dependon 𝑧when 𝐸and∇𝑇are parallel to 𝑂𝑍. In this way, the three-dimensional problem is reduced to a quasi-one-dimensional one, with an infinite set of identical elements of area 𝐴conducting heat in parallel, and Eq. (4.5) remains valid for obtaining 𝜅𝑙if an appropriate transmission per unit area is defined. A process similar to the one leading to Eq. (4.35) can be followed to yield expressions for 𝜎,𝑆and 𝜅𝑒. At equilibrium, electrons are distributed among the available states according to the Fermi-Dirac distribution 𝑓𝐹𝐷(𝜖)=1 𝑒𝜖−𝜇 𝑘𝐵𝑇+1,(5.6) where 𝜖denotes the energy of each state and 𝜇the chemical potential. The measured electric field [137] is given by the gradient of the electrochemical potential, i.e.,𝐸(𝑧)=−𝜕􀊂𝜙−𝜇/ℯ􀊅/𝜕𝑧, where the electrostatic potential is represented by 𝜙and the elementary charge by ℯ. In a linear non-equilibrium regime, at each 𝑧the steady-state distribution canbe decomposed ina sum of 𝑓𝐹𝐷evaluated at the localtemperature 𝑇(𝑧)and electrostatic potential 𝜙(𝑧)and a small perturbation. For electrons in band ♢ with a momentum ℏ𝑘and a velocity 𝑣♢=􀊂𝜕𝜖♢/𝜕𝑘􀊅/ℏ, 𝑓􀊂𝑧;𝑘,♢􀊅=𝑓𝐹𝐷􀊂𝑇(𝑧),𝜙(𝑧);𝑘,♢􀊅+𝑔􀁮􀊂𝑧;𝑘,♢􀊅, with 􀉤𝑔􀁮􀉤≪􀉤𝑓𝐹𝐷􀉤,(5.7) and the Boltzmann transport equation adopts the form 𝑣(𝑧) ♢⎡⎢⎢⎣𝜕𝑓𝐹𝐷􀊂𝑇,𝜙;𝑘,♢􀊅 𝜕𝑇 𝜕𝑇 𝜕𝑧+𝜕𝑓𝐹𝐷􀊂𝑇,𝜙;𝑘,♢􀊅 𝜕𝜖 ℯ𝐸(𝑧)⎤⎥⎥⎦=−𝑔􀁮􀊂𝑧;𝑘,♢􀊅 𝜏♢(5.8) in the relaxation time approximation, by arguments analogous to those preceding Eq. (4.33), but taking the electric field into account. Due to the form of 𝑓𝐹𝐷,𝜕𝑓𝐹𝐷/𝜕𝑇is proportional to 𝜕𝑓𝐹𝐷/𝜕𝜖through a factor 􀊂𝜇−𝜖􀊅/(𝑘𝐵𝑇), so 𝑔􀁮􀊂𝑧;𝑘,♢􀊅=−𝜏♢𝑣(𝑧) ♢𝜕𝑓𝐹𝐷􀊂𝑇,𝜙;𝑘,♢􀊅 𝜕𝜖 􀊄ℯ𝐸(𝑧)−𝜖♢−𝜇 𝑘𝐵𝑇𝜕𝑇 𝜕𝑧􀊇.(5.9) 89 5. Thermoelectric properties of hybrid organic-inorganic superlattices Justas inthe case ofphonons, only this perturbationwith respecttoequilibrium has to be considered when computing the net currents. The contribution of each electron to 𝑗(𝑧)is simply −𝑒𝑣(𝑧), while its share of 𝑗(𝑧) 𝑄can be obtained by subtracting its chemical potential (which cannot be identified as heat, being associated to a deformation coordinate, namely the number of particles) from the total energy it carries and multiplying by its velocity, with the result 􀊂𝜖−𝜇􀊅𝑣(𝑧). Summing over all available 𝑘-points per unit volume (i.e., integrating these contributions over the Brillouin zone and dividing by 8𝜋􀁰) and over bands, the following expressions for the net currents are found 𝑗(𝑧)=􀈪 ♢􀈧 𝐵𝑍 −ℯ𝑣(𝑧) ♢􀊂𝑘􀊅𝑔􀁮􀊂𝑘,♢􀊅𝑑􀁰𝑘 8𝜋􀁰=𝐸(𝑧)⎧⎪⎨⎪⎩􀈪 ♢􀈧 𝐵𝑍 ℯ􀁯𝑣(𝑧) ♢􀊂𝑘􀊅𝛬♢􀊂𝑘􀊅𝜕𝑓𝐹𝐷 𝜕𝜖 𝑑􀁰𝑘 8𝜋􀁰⎫⎪⎬⎪⎭+ +𝜕𝑇 𝜕𝑧⎧⎪⎨⎪⎩−􀈪 ♢􀈧 𝐵𝑍 ℯ𝜖♢􀊂𝑘􀊅−𝜇 𝑘𝐵𝑇𝜕𝑓𝐹𝐷 𝜕𝜖 𝑑􀁰𝑘 8𝜋􀁰⎫⎪⎬⎪⎭(5.10a) 𝑗(𝑧) 𝑄=􀈪 ♢􀈧 𝐵𝑍 􀉼𝜖♢􀊂𝑘􀊅−𝜇􀉿𝑣(𝑧) ♢􀊂𝑘􀊅𝑔􀁮􀊂𝑘,♢􀊅𝑑􀁰𝑘 8𝜋􀁰= =𝐸(𝑧)⎧⎪⎨⎪⎩−􀈪 ♢􀈧 𝐵𝑍 ℯ􀉼𝜖♢􀊂𝑘􀊅−𝜇􀉿𝑣(𝑧) ♢􀊂𝑘􀊅𝛬♢􀊂𝑘􀊅𝜕𝑓𝐹𝐷 𝜕𝜖 𝑑􀁰𝑘 8𝜋􀁰⎫⎪⎬⎪⎭ +𝜕𝑇 𝜕𝑧⎧⎪⎪⎨⎪⎪⎩􀈪 ♢􀈧 𝐵𝑍 􀉼𝜖♢􀊂𝑘􀊅−𝜇􀉿􀁯 𝑘𝐵𝑇𝜕𝑓𝐹𝐷 𝜕𝜖 𝑑􀁰𝑘 8𝜋􀁰⎫⎪⎪⎬⎪⎪⎭.(5.10b) Clearly, expressions for 𝜎,𝑆and 𝜅𝑒can be extracted from these equations by comparison with Eqs. (5.4). Defining 𝑟≔(𝑘𝐵𝑇)−􀁮􀊂𝜖−𝜇􀊅and performing some simple algebraic transformations, they can be cast in the following convenient forms [186] 𝜎=ℯ􀁯􀈧𝒮􀊂𝑘𝐵𝑇𝑟+𝜇􀊅􀊄−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊇𝑑𝑟 (5.11a) 𝑇𝜎𝑆=𝑘𝐵𝑇ℯ􀈧𝑟𝒮􀊂𝑘𝐵𝑇𝑟+𝜇􀊅􀊄−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊇𝑑𝑟 (5.11b) 𝜅𝑒+𝑇𝜎𝑆􀁯=𝑘􀁯 𝐵𝑇􀈧𝑟􀁯𝒮􀊂𝑘𝐵𝑇𝑟+𝜇􀊅􀊄−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊇𝑑𝑟, (5.11c) 90 5.3. Transmission calculations with 𝒮(𝜖)≔􀈪 ♢􀈧 𝐵𝑍 𝑣(𝑧) ♢􀊂𝑘􀊅𝛬♢􀊂𝑘􀊅𝛿􀉼𝜖−𝜖♢􀊂𝑘􀊅􀉿𝑑􀁰𝑘 8𝜋􀁰.(5.11d) In the next section some simplifications will be assumed in order to arrive at even more tractable expressions. It must be noted that, although in this deduction the charge carriers have been assumed to be electrons, all the results are readily applicable to holes if the appropriate signs are changed. 5.3. Transmission calculations Three steps are needed in order to be able to perform the electric and thermal calculations: model the semiconducting part, characterise the molecule, and combine the two parts in a sensible fashion. SiGe is a well-known material, so good parameterisations are readily available for it in the scientific literature. As regards charge carrier behaviour, the model employed for SiGe alloys comprised a single parabolic valence band and two conduction bands (L, with six equivalent parabolic minima, and X, with four). The required band parameters where taken from Refs. 187 and 188. For each band, an energy-independent relaxation time was assumed [188] with two contributions, bulk and alloy scattering, compounded using Matthiessen’s rule: 𝜏♢=𝑚𝑐,♢ ℯ1 𝜇−􀁮 􀂏􀂢􀂙􀂘+𝜇−􀁮 􀂎􀂙􀂙􀂜􀂦 (5.12a) 𝜇􀂏􀂢􀂙􀂘 =􀊄8.6⋅10−􀁰 m􀁯 Vs􀊇(1−𝑥)+􀊄4.07⋅10−􀁰 m􀁯 Vs􀊇𝑥(5.12b) 𝜇􀂎􀂙􀂙􀂜􀂦 =1.6⋅10−􀁯 􀂚􀁹 􀃵􀂠 4𝑥(1−𝑥)􀇽𝑇 􀁰􀁭􀁭􀃪,(5.12c) where 𝑚𝑐denotes the conduction effective mass of each band and 𝑥is the fraction of silicon in the alloy. Under these hypotheses, the electric conductivity of SiGe, its Seebeck coefficient and the contribution of charge carriers to its thermal conductivity can be calculated as: 91 5. Thermoelectric properties of hybrid organic-inorganic superlattices 𝜎=2ℯ􀁯 ℎ􀈧􀊄−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊇𝛱(𝑟)𝑑𝑟 (5.13a) 𝑆=𝑘𝐵∫􀊃−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊆𝑟𝛱(𝑟)𝑑𝑟 ∫􀊃−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊆𝛱(𝑟)𝑑𝑟 (5.13b) 𝜅𝑒=2𝑘􀁯 𝐵𝑇 ℏ􀈧􀊄−𝑑𝑓𝐹𝐷 𝑑𝑟 􀊇𝑟􀁯𝛱(𝑟)𝑑𝑟−𝑇𝜎𝑆􀁯(5.13c) with 𝛱(𝑟)=√8 3𝜋ℏ⎡⎢⎢⎢⎢⎣􀈪 ♢∈ 􀂐􀂜􀂛􀂑􀂢􀂐􀂡􀂖􀂜􀂛 􀂏􀂎􀂛􀂑􀂠 𝑁♢𝜏♢𝛩􀊂𝑘𝐵𝑇𝑟+𝜇−𝜖􀁭,♢􀊅􀇾𝑚∗♢􀊂𝑘𝐵𝑇𝑟+𝜇−𝜖􀁭,♢􀊅􀁰+ +𝜏􀂣􀂎􀂙𝛩􀊂𝜖􀁭,􀂣􀂎􀂙−𝑘𝐵𝑇𝑟−𝜇􀊅􀇾𝑚∗􀁭􀊂𝜖􀁭,􀂣􀂎􀂙−𝑘𝐵𝑇𝑟−𝜇􀊅􀁰⎤⎥⎥⎦,(5.13d) simplified versions of Eqs. (5.11) with the integration around each parabolic minimum solved analytically. Here, 𝑁is the number of equivalent minima in each band, 𝑚∗the corresponding density-of-states effective mass, 𝜖􀁭the energy of the band edge and 𝛩a step function. Band parameters are listed in Table 5.1. By comparing these equations to the one-dimensional result for the thermal conductivity (4.5) or, more generally, to the Landauer-Buttiker formalism for electrons [17], built upon similar premises, it can be seen that they are also applicable to a bidimensional array of quasi-one-dimensional conducting elements such as a molecular monolayer if 𝛱is replaced with 𝜌𝑆𝐿𝒯𝑒,i.e., the product of the electronic transmission of each element (𝒯𝑒), the surface density of elements (𝜌𝑆) and the width of the layer (𝐿). Thus, 𝛱can be thought of as a bulk analogue of the transmission; knowledge of 𝛱for a given material is sufficient to calculate its thermoelectric power factor 𝑃=𝜎𝑆􀁯and, if the phononic contribution to its thermal conductivity can be estimated, also its thermoelectric figure of merit. With respect to the thermal transmission of SiGe, it was provided by Dr. Natalio Mingo, who calculated it in a simplified way by the use of an approximate linear phonon dispersion — a Debye model with a carefully selected cutoff frequency — and parameterised relaxation times [189] that take into account anharmonic and alloy scattering. 92 5.3. Transmission calculations Table 5.1 Parameters for each band in SiGe, from Refs. 187 and 188. Here, 𝑚􀁭is the electron mass; for non-rotationally-symmetric paraboloids, 𝑚𝑙and 𝑚𝑡are the longitudinal and transverse effective masses, respectively. ♢(Band) 𝑚𝑙,♢/𝑚􀁭𝑚𝑡,♢/𝑚􀁭𝑚𝑐,♢/𝑚􀁭𝑚∗♢/𝑚􀁭 X0.97 0.19 3􀊂𝑚􀁭/𝑚𝑙,𝑋+2𝑚􀁭/𝑚𝑡,𝑋􀊅􀁺 􀇽𝑚𝑙,𝑋𝑚􀁯 𝑡,𝑋/𝑚􀁭 L 1.64 0.082 3􀊂𝑚􀁭/𝑚𝑙,𝐿+2𝑚􀁭/𝑚𝑡,𝐿􀊅􀁺 􀇽𝑚𝑙,𝐿𝑚􀁯 𝑡,𝐿/𝑚􀁭 Valence 1 1 1 1 Gap widths (eV):􀊊𝜖𝑔,𝑋 =0.8941+𝑥(0.0421+0.1691𝑥) 𝜖𝑔,𝐿 =0.7596+𝑥(1.0860+0.3306𝑥). The percentage of germanium in the SixGe1-x alloy plays a crucial role in the modulation of the thermoelectric properties of the superlattice. Compared to pure silicon, an alloy with significant disorder scatters both electrons and phonons more efficiently. In order to evaluate the net effect of this parameter, calculations were run for the two most extreme cases: 𝑥=1(no germanium) and 𝑥=0.5(maximum disorder). The position of the Fermi level (𝜖𝐹) was chosen so as to maximise the power factor 𝑃=𝜎𝑆􀁯, which happens close to the edge of the conduction band and yields carrier densities 𝑛∼10􀁯􀁭 cm−􀁰. A superlattice whose semiconducting part is made of pure silicon proved a poor choice for thermoelectric applications. Therefore, the discussion in the next section will concentrate on the maximally-disordered, optimally-doped SiGe:SAM HOI. The organic molecules were modelled atomistically by Prof. Hans Ågren and coworkers. They used density functional theory (DFT) calculations at the B3LYP level [190] with the 6-31G basis set in order to get the optimised geometries and electronic structures of SiH3-tri-thiophene-SiH3, GeH3-tri-thiophene- GeH3, SiH3-phenyl-tri-thiophene-SiH3and GeH3-phenyl-tri-thiophene-GeH3 molecules. All of the quantum chemical calculations were performed with GAUSSIAN 09 [191]. In DFT [192], electrons are described not in terms of their wave functions, but of their total charge density which, according to the Hohenberg-Kohn theorems [193], contains all the physics of the system. This charge density is, in turn, calculated by solving the Kohn-Sham equations 93 5. Thermoelectric properties of hybrid organic-inorganic superlattices [194], formally identical to the time-independent Schrödinger equation 𝑯􀉤𝜓􀈊=𝜖􀉤𝜓􀈊(5.14) but describing a set of fictitious, non-interacting electrons. This difference is reflected in the form of the hamiltonian (𝑯), which contains exchange and correlation contributions to the potential energy to account for the collective effect of all the other electrons. Nuclear coordinates are typically decoupled from electronic degrees of freedom and treated in the Born-Oppenheimer approximation [195]. The force associated to atomic coordinate 𝑥􀊂𝜇􀊅 𝑗is defined, as usual, by 𝑓􀊂𝜇􀊅 𝑗=−𝜕𝜖/𝜕𝑥􀊂𝜇􀊅 𝑗, but advantage can be taken of the Hermitian nature of 𝑯, through a process analogous to the one leading to Eq. (3.8) for group velocities, to obtain a more convenient expression, 𝑓􀊂𝜇􀊅 𝑗=−􀈙𝜓􀉧􀉧𝜕𝑯 𝜕𝑥􀊂𝜇􀊅 𝑗􀉧􀉧𝜓􀈌,(5.15) known as the Hellman-Feynman theorem [196]. For this work, the numerical derivative of these forces was computed using Eq. (3.9); however, it should be mentioned that an alternative algorithm exists [197, 198] to solve the problem directly in terms of the hamiltonian in the framework of density functional perturbation theory (DFPT), of which Eq. (5.15) can be considered a particular application. Since force constants obtained by DFT methods do not come from a shortrange potential, they are seldom directly usable in phononic calculations. For instance, conservation of momentum (or, equivalently, translational symmetry) demands that all the components of the total harmonic force on the whole system, ∑ 𝜇,𝜇′,𝑗,𝑗′𝐾􀊂𝜇,𝜇′􀊅 𝑗,𝑗′𝑢􀊂𝜇′􀊅 𝑗′, be zero, which is only possible if ∑ 𝜇′,𝑗′𝐾􀊂𝜇,𝜇′􀊅 𝑗,𝑗′=0 for every atom 𝑗along every direction 𝜇. Similar linear constraints on the elements of 𝑲can be derived from the conservation of angular momentum. Force constants derived from DFT can deviate from these constraints quite significantly; if used to calculate the vibrational frequencies of a molecule, they would fail to predict the 𝜔=0modes associated to translations and rotations, while if used to calculate its transmission along the 𝑂𝑍axis when attached to two leads, they would yield a value smaller than the theoretical 𝒯(0)=4due to such modes. When it is not feasible to use a larger simulation box in order to avoid this effect, 𝑲may be corrected using a method devised by Mingo 94 5.3. Transmission calculations Table 5.2 Parameters of the SW potential for Ge, from Ref. 146. 𝜎=0.2181nm 𝜖=1.93eV 𝐴=7.049556277 𝐵=0.6022245584 𝑎=1.80 𝜆=31.0 𝑝=4 𝑞=0 𝛾=1.20 and Broido [199], which enforces the symmetries while keeping the relative correction to the force constants minimal, through a Lagrange-multiplier approach. In practical terms, this translates into the problem of finding the solution of a relatively large linear system, which can be accomplished more efficiently than a larger DFT calculation. Thus, it was the method chosen for the present work. The phononic transmission of the molecular layer was computed considering a single molecule between pure Si or pure Ge leads with the same methods from Chapter 4. The force constant matrix of the defective system (semiconductor leads+molecule) was built by parts: the corrected force constants from DFT were used for the molecule and for the force between the molecule and the leads, whereas semiconductor-semiconductor interactions were again modelled using the SW potential [43, 146], with the parameters for Si of Table 4.1 and those listed in Table 5.2 for Ge. An added advantage of this was that Green’s functions obtained by decimation [140] for the previous chapter were reused. The cross-sectional area of the nanowire studied there was deemed enough to yield a transmission per unit area representative of a molecule attached to the bulk. The electronic transmission probabilities across the molecular interface were calculated with the QCME (Quantum Chemistry for Molecular Electronics) program [200], which is based on the general Green’s function formalism [201, 202]. QCME has been successfully applied to describe the electronic transport properties of various molecular junction systems [203–205]. In their calculations, Ågren and coworkers divided the molecular junction into three parts: source, extended molecule, and drain. The source and drain electrodes were described by an effective mass approximation, while the electronic structure of the extended molecule was calculated with DFT. With such a setup, they were able to accurately describe both the bulk electrodes and the extended molecule. In the framework of elastic-scattering theory, the 95 5. Thermoelectric properties of hybrid organic-inorganic superlattices Figure 5.6 Room-temperature power factor of a Si0.5Ge0.5/tri-thiophene superlattice as a function of its period length, using ohmic and ballistic composition rules for the electronic calculations, with or without a side phenyl group. 101102103 l+L(nm) 0 2 4 6 8 10 PµW cm K2 Ohmic, no side group Ohmic, with side group Ballistic, no side group Ballistic, with side group coupling regimes. Although it seems unlikely that the ballistic picture affords good results for 𝑙+𝐿as large as 10nm, even if it only held up to a fifth of that value it would still yield 𝑍𝑇≃0.23. At the other extreme, a very long period (∼0.2−0.3μm) maximises the figure of merit in the ohmic regime, with a similar optimum value. A third interesting conclusion which can be drawn from Fig. 5.7 is that thermoelectric properties are easily tunable by chemical methods. The phenyl group marks a significant 20%difference in the optimum 𝑍𝑇in the ohmic regime, and a huge departure of almost 100%for ballistic coupling, by virtue of affecting the phononic and electronic transmission profiles to very different degrees. The almost infinite flexibility offered by organic molecules for substitution with different residues, different choices of the length of the oligomer, etc., therefore appears as a promising avenue for improving 𝑍𝑇even further. At the current stage of technological development, these methods are possibly more economical and easily scalable to industrial sizes than other alternative routes dependent on nanoscale material engineering [130]. Therefore, these calculations reveal that, whereas when the inorganic part 102 5.4. Results and discussion Figure 5.7 Room-temperature figure of merit of a Si0.5Ge0.5/tri-thiophene superlattice as a function of its period length, using ohmic (left) and ballistic (right) composition rules for the electronic calculations. 101102103 l+L(nm) 0.00 0.05 0.10 0.15 0.20 0.25 0.30 ZT ZT (310 nm)= 0.24 ZT (230 nm)= 0.20 No side group With side group 0246810 l+L(nm) ZT (10 nm)= 0.27 ZT (10 nm)= 0.14 consists of pure silicon the thermoelectric behaviour of the resulting structure is rather poor, an alloy with a percentage of Si around 50%, leading to a maximal configurational entropy, offers promising results. In particular, as regards electric transport, it is found that the organic layers significantly reduce the conductivity with respect to that of bulk SiGe. Nevertheless, since it was also detected that thermal conductivity is reduced by a much larger factor [resulting in values in the order of magnitude from 0.1to 1W/(mK)], the thermoelectric figure of merit (𝑍𝑇) of this kind of hybrid structure can improve upon that of SiGe alone by a factor of more than two. Optimal values of 𝑍𝑇around 0.25were achieved at room temperature (∼2.5times larger than for bulk SiGe), which could make this kind of material competitive for practical thermoelectric applications if, as expected, they are easier to engineer and manufacture than other, more sophisticated, nanostructures. Moreover, the addition of a phenyl ring to each polymer alters the value of 𝑍𝑇by about 20%, which suggests that the thermoelectric properties of these systems can be easily tailored and improved by chemical methods. 103 5. Thermoelectric properties of hybrid organic-inorganic superlattices References 17. Datta, S. Quantum Transport: Atom to Transistor second (Cambridge University, New York, 2005). 43. Stillinger, F. H. & Weber, T. A. Phys. Rev. B 31, 5262 (1985). 130. Hochbaum, A. I., Chen, R., Delgado, R. D., Liang, W., Garnett, E. C., Najarian, M., Majumdar, A. & Yang, P. Nature (London) 451, 163 (2008). 137. Ziman, J. M. Electrons and Phonons (Oxford University, New York, 1960). 140. Guinea, F., Tejedor, C., Flores, F. & Louis, E. Phys. Rev. B 28, 4397 (1983). 146. Jian, Z., Kaiming, Z. & Xide, X. Phys. Rev. B 41, 12915 (1990). 155. Carnot, S. Réflexions sur la Puissance Motrice du Feu (Bachelier, Paris, 1824). 156. Snyder, G. J. & Ursell, T. S. Phys. Rev. Lett. 91, 148301 (2003). 157. DiSalvo, F. J. Science 30, 703 (1999). 158. Venkatasubramanian, R., Siivola, E., Colpitts, T. & O’Quinn, B. Nature 413, 597 (2001). 159. Leclerc, M. & Najari, A. Nat. Mater. 10, 409 (2011). 160. Dubey, N. & Leclerc, M. J. Polym. Sci., Part B: Polym. Phys. 49, 467 (2011). 161. Sanchez, C. J. Mater. Chem. 15, 3557 (2005). 162. Mitzi, D. B. Chem. Mater. 13, 3283 (2001). 163. Xing, L.-L., Li, D.-P., Hu, S.-X., Jing, H.-Y., Fu, H., Mai, Z.-H. & Li, M. J. Am. Chem. Soc. 128, 1749 (2006). 164. Yoon, K.-H., Han, K.-S. & Sung, M.-M. Nanoscale Res. Lett. 7, 71 (2012). 165. Deneke, C., Zschieschang, U., Klauk, H. & Schmidt, O. G. Appl. Phys. Lett. 89, 263110 (2006). 166. Deneke, C., Schumann, J., Engelhard, R., Thomas, J., Sigle, W., Zschieschang, U., Klauk, H., Chuvilin, A. & Schmidt, O. G. Phys. Status Solidi C5, 2704 (2008). 167. Bufon, C. C. B., Espinoza, J. D. A., Thurmer, D. J., Bauer, M., Deneke, C., Zschieschang, U., Klauk, H. & Schmidt, O. G. Nano Lett. 11, 3727 (2011). 168. Mitzi, D. B., Chondroudis, K. & Kagan, C. R. IBM Res. Dev. 45, 29 (2001). 104 References 169. Kagan, C. R., Mitzi, D. B. & Dimitrakopoulos, C. D. Science 286, 945 (1999). 170. Carrasco-Orozco, M. A., Stirner, T., O’Neill, M., Ellis, C., Dong, D., Kelly, R., Piepenbrock, M. O. & Kelly, S. M. Phys. Rev. B 75, 035207 (2007). 171. Park, Y., Han, K. S., Lee, B. H., Cho, S., Lee, K. H., Im, S. & Sung, M. M. Org. Electron. 12, 348 (2010). 172. See, K. C., Feser, J. P., Chen, C. E., Majumdar, A., Urban, J. J. & Segalman, R. A. Nano Lett. 10, 4664 (2010). 173. Malen, J. A., Doak, P., Baheti, K., Tilley, T. D., Majumdar, A. & Segalman, R. A. Nano Lett. 9, 3406 (2009). 174. Ke, S.-H., Yang, W., Curtarolo, S. & Baranger, H. U. Nano Lett. 9, 1011 (2009). 175. Yan, L., Shao, M., Wang, H., Dudis, D., Urbas, A. & Hu, B. Adv. Mater. 23, 4120 (2011). 176. D. Appelhansa, a. D. F., Adlera, H., Pliethb, W., Fikusb, A., Grundkec, K., Schmittc, F., Bayerc, T. & Adolphid, B. Colloids Surf., A 161, 203 (2000). 177. Sathyapalan, A., Ng, S. C., Lohani, A., Ong, T. T., Chen, H., Zhang, S., Lam, Y. M. & Mhaisalkar, S. G. Thin Solid Films 516, 5645 (2008). 178. Fabre, B., Lopinski, G. P. & Wayner, D. D. M. Chem. Commun. 2002, 2904 (2002). 179. de Groot, S. R. & Mazur, P. Non-Equilibrium Thermodynamics (Dover, New York, 1984). 180. Onsager, L. Phys. Rev. 37, 405 (1931). 181. Hill, T. L. Thermodynamics of Small Systems (Benjamin, New York, 1963). 182. Letellier, P., Mayaffre, A. & Turmine, M. Phys. Rev. B 76, 045428 (2007). 183. Carrete, J., Varela, L. M. & Gallego, L. J. Phys. Rev. E 77, 022102 (2008). 184. Seebeck, T. J. Abh. K. Akad. Wiss. 2, 265 (1823). 185. CRC Handbook of Thermoelectrics 1st ed. (ed Rowe, D. M.) (CRC Press, Boca Raton, 1995). 186. Mahan, G. D. & Sofo, J. O. Proc. Natl. Acad. Sci. USA 93, 7436 (1996). 187. Krishnamurthy, S., Sher, A. & Chen, A. Appl. Phys. Lett. 47, 160 (1985). 188. Slack, G. A. & Hussain, M. A. J. Appl. Phys. 47, 2694 (1991). 105 5. Thermoelectric properties of hybrid organic-inorganic superlattices 189. Mingo, N., Hauser, D., Kobayashi, N. P., Plissonnier, M. & Shakouri, A. Nano Lett. 9, 711 (2009). 190. Kim, K. & Jordan, K. D. J. Phys. Chem. 98, 10089 (1994). 191. Frisch, M. J. et al. Gaussian 09 Revision A.02 Gaussian Inc. Wallingford CT 2009. 192. Parr, R. G. & Yang, W. Density Functional Theory of Atoms and Molecules (Oxford University Press, New York, 1989). 193. Hohenberg, P. & Kohn, W. Phys. Rev. 136, B864 (1964). 194. Kohn, W. & Sham, L. J. Phys. Rev. 140, A1133 (1965). 195. Born, M. & Oppenheimer, R. Ann. Phys. 84, 459 (1927). 196. Feynman, R. P. Phys. Rev. 56, 340 (1939). 197. Gonze, X., Allan, D. C. & Teter, M. P. Phys. Rev. Lett 68, 3603 (1992). 198. Gonze, X. Phys. Rev. A 52, 1086 (1995). 199. Mingo, N., Stewart, D. A., Broido, D. A. & Srivastava, D. Phys. Rev. B 77, 033418 (2008). 200. Jiang, J. & Luo, Y. QCME-V1.0 (Quantum Chemistry for Molecular Electronics) Royal Institute of Technology, Sweden, 2005. 201. Wang, C.-K., Fu, Y. & Luo, Y. Phys. Chem. Chem. Phys. 3, 5017 (2001). 202. Jiang, J., Kula, M. & Luo, Y. J. Chem. Phys. 124, 034708 (2006). 203. Hu, W., Jiang, J., Nakashima, H., Luo, Y., Kashimura, Y., Chen, K.-Q., Shuai, Z., Furukawa, K., Lu, W., Liu, Y., Zhu, D. & Torimitsu, K. Phys. Rev. Lett. 96, 027801 (2006). 204. Su, W. Y., Jiang, J., Lu, W. & Luo, Y. Nano Lett. 6, 2091 (2006). 205. Cao, H., Jiang, J., Ma, J. & Luo, Y. J. Am. Chem. Soc. 130, 6674 (2008). 206. Vining, C. B. J. Appl. Phys. 69, 331 (1991). 207. Savić, I., Mingo, N. & Stewart, D. A. Phys. Rev. Lett. 101, 165502 (2008). 208. Chiritescu, C., David G. Cahill and, N. N., Johnson, D., Bodapati, A., Keblinski, P. & Zschack, P. Science 315, 351 (2007). 209. Schaffler, F. in. Properties of Advanced Semiconductor Materials GaN, AlN, InN, BN, SiC, SiGe (eds Levinshtein, M. E., Rumyantsev, S. L. & Shur, M. S.) 149 (Wiley, New York, 2001). 106 Part II Ionic liquids 107 6Nanostructure of imidazolium-based ionic liquids And yet it is hard to believe that anything in nature could stand revealed as solid matter. The lightning of heaven goes through the walls of houses, like shouts and speech; iron glows white in fire; red-hot rocks are shattered by savage steam; hard gold is softened and melted down by heat; chilly brass, defeated by heat, turns liquid; heat seeps through silver, so does piercing cold; by custom raising the cup, we feel them both as water is poured in, drop by drop, above. De Rerum Natura Lucretius 6.1. Introduction Ionic liquids (ILs) are substances present in the liquid state and formed exclusively by ions at room temperature. In practice, a substance is usually considered an IL if it is fully dissociated and its melting temperature lies below 100∘C. If the latter requirement were lifted, ordinary molten salts, like liquid 109 6. Nanostructure of imidazolium-based ionic liquids NaCl, would also enter the category. This second kind of substances, corrosive and very viscous, share certain characteristics with ILs, but their much higher melting point clearly separates their domain of usefulness from that of the latter, which is the main reason behind their separate treatment. An IL is formed by an organic cation, whose complexity can vary, and an anion which can range from a single halogen atom to another complex organic structure. The first documented synthesis of an IL, ethylammonium nitrate, was reported in 1914 [210, 211], and the first systematic experimental description of one of these systems dates from 1948 [212], although interest in ILs for use as solvents emerged in the 80s [213, 214]. Another key moment was the synthesis by Wilkes, in the 90s, of ILs based on weakly coordinating ions, more economical than those available up to that point [215]. ILs are singular in their structure and dynamics, which confers them an important theoretical appeal, but without a doubt their popularity is due to their great practical usefulness as solvents, reaction media and catalysts of multiple chemical reactions [12–14]. The main properties that make them especially suitable for such purposes are: ▶Their low vapour pressure: as a matter of fact, this pressure is so low as to be undetectable in most measurements. A liquid which essentially does not evaporate is easy to manipulate without losses to the environment, and to separate from certain solutes using energetically inexpensive procedures. Thus, sometimes ILs are referred to as “green solvents”, even though this point has to be qualified, since their syntheses can be environmentally wasteful and some of them are toxic [216]. ▶Their wide range of work temperatures: an intelligent choice of ions can result in ILs with a melting temperature anywhere between −90∘Cand 200∘C. The other extreme of the temperature range is defined by the compound’s thermal decomposition temperature, which can be as high as 400∘C[217]. As a consequence, these liquids are ideal media for many chemical processes at different temperatures. A particular group of ILs with the added property of a great chemical stability is that formed by those whose cation is based on an imidazole — or 1,3-diazacyclopenta-2,4-diene — ring. As can be deduced from its systematic name, this is a pentagonal carbon ring with two of its atoms, in non-adjacent sites, substituted by nitrogen atoms. In imidazole, those bonds not responsible 110 6.1. Introduction Figure 6.1 From left to right: imidazolium, [BMIM]+, [PF6]–and [BF4]–. for the pentagonal structure are saturated by hydrogen, yielding the formula C3H4N2. If a methyl group and a generic alkyl chain are bound to the nitrogen atoms instead, the family of 1-alkyl-3-methylimidazoles is obtained. In order to avoid the repetition of such a verbose notation, the most common members of this family are referred to as DMIM (1,3-dimethylimidazole), EMIM (1-ethyl-3-methylimidazole), BMIM (1-buthyl-3-methylimidazole), HMIM (1- hexyl-3-methylimidazole), MOIM (1-methyl-3-octylimidazole), etc. A less often seen but still common notation is based on specifying the number of carbons in the alkyl chain: C6MIM instead of HMIM, for instance. Following the first of these conventions, [BMIM]+is 1-buthyl-3-methylimidazolium, the monovalent cation resulting from ionisation of BMIM. Some of the most frequentcounterionsarehexafluorophosphate([PF6]–), tetrachloroborate([BF4]–) and halogens such as chloride (Cl–). Although the theoretical aspects in Part II of this thesis will try to be as general as possible, whenever specific examples are needed, most often they will be imidazolium-based ILs, since they are widely used in industry and there are force fields parameterised specifically for them and tested in MD simulations [218, 219]. An imidazolium ring, along with the [BMIM]+, [PF6]–and [BF4]–ions, is represented in Fig. 6.1. 111 6. Nanostructure of imidazolium-based ionic liquids Figure 6.2 Top: cation-anion, cation-cation and anion-anion RDFs in pure [BMIM][BF4]. The dashed line marks the cut-off distance taken for considering two ions as connected. Bottom: oxygen-oxygen RDFs in pure water, ethanol and methanol. 0.0 0.5 1.0 1.5 2.0 2.5 r(nm) 0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.5 g(r) C2−B C2−C2 B−B 0.0 0.2 0.4 0.6 0.8 1.0 1.2 1.4 1.6 r(nm) 0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.5 4.0 4.5 g(r) O−O, water O−O, methanol O−O, ethanol were analysed. Following the criterion defined by Hanke and Lynden-Bell [239] and later employed by Bernardes et al. [240], it was considered that two molecules of water or alcohol are connected to each other and thus belong to the same cluster if the distance between their oxygen atoms is smaller than the radius corresponding to the first minimum in the oxygen-oxygen radial distribution function [RDF, 𝑔(𝑟)] in the pure liquids (Fig. 6.2, bottom). This is the limit of the first solvation layer, and corresponds approximately to the distance used to define a hydrogen bond in the geometrical criterion commonly employed in MD (hydrogen-acceptor distance smaller than 3.5 A, and donor-hydrogen-acceptor angle less than 30∘[261]). The criterion used to define ionic clusters is slightly different. Heterocoordination between cations and anions is the norm in ILs due to its energetic advantages; therefore, the distance considered as the cut-off was 0.65nm, which is the distance where the cation-anion and cation-cation RDFs of pure 118 6.3. Results and discussion Figure 6.3 Solvent concentration dependence of the percentage of ions (left panels) and solvent molecules (right panels) forming clusters and big clusters in mixtures of [BMIM][BF4] with water (top), methanol (centre) and ethanol (bottom). Solid circles mark the simulated concentrations; lines are provided only as guides to the eye. 0 20 40 60 80 100 In clusters In big clusters 0 20 40 60 80 100 0 20 40 60 80 100 0 20 40 60 80 100 0 20 40 60 80 100 % of ions Solvent concentration (%) % of solvent molecules [BMIM][BF4] intersect (Fig. 6.2, top), and accordingly the minimum distance at which it is more likely to find a second cation after a cation-anion pair. These RDFs were calculated using the boron atom (B), at the centre of mass of [BF4]–, as representative of the anion, and the carbon atom between the two nitrogens (C2) as representative of the imidazolium ring. It should be noted that these cut-off distances remain unaffected when the solvent concentration is varied. For eachframealong the MDtrajectory, asearch was performed to buildthe connectivitymatrix of an undirected network representing theneighbourhood relationsofsolvent molecules or ions in themixtureatthatparticulartimestep, according to the cut-off radii previously chosen. Clusters were then defined as the connected components of that undirected graph. The cluster distribution of each mixture was obtained by taking into account the clusters formed at all time steps in the simulation. Big clusters were arbitrarily defined, for the purposes of the present work, as those that comprise more than 50%of the particles belonging to the class under study (either solvent molecules or ionic pairs) in the simulation box. Figure 6.3 shows the evolution of the percentage of water, methanol and 119 6. Nanostructure of imidazolium-based ionic liquids ethanol molecules, respectively, that belong to a cluster (i.e., which are not isolated) and to a big cluster. As Fig. 6.3 (top left) shows, all the ions belong to big clusters up to a water molar percentage of 90%; after this concentration, the number of cations and anions forming clusters decreases when the amount of water is increased. However, in mixtures with methanol and ethanol (Fig. 6.3, centre left and bottom left, respectively) the percentage of ions in big clusters starts to decrease at an alcohol concentration of 80%. In regard to solvent clusters, the percentage of water molecules that belong to a cluster increases rapidly with the amount of water (Fig. 6.3, top right): indeed, at a molar percentage of approximately 35%half of the water molecules belong to a cluster, and when 80%of water is reached more than 80%of the water molecules are forming big clusters. The behaviour of alcohol molecules is markedly different: firstly, the increase with alcohol concentration of the number of solvent molecules belonging to a cluster (Fig. 6.3, centre right and bottom right) is much slower than in the case of water. Even at 70%alcohol, half of the alcohol molecules still do not belong to any cluster. Methanol molecules start to form big clusters in a significant number at very high alcohol concentrations (99% and above) but those clusters are conspicuously absent from [BMIM][BF4] + ethanol mixtures. Further insight into the modifications introduced by a solvent in the clustering process of [BMIM][BF4] is given by the size distribution histograms of ionic and solvent clusters for each of the systems. Figure 6.4 shows the probability of finding an ion or a molecule of water in an aggregate comprising a given percentage of the particles in the simulation box for three different water concentrations. Solid dots show the actual cluster sizes 𝑛in order 𝑛=1, 𝑛=2… The same quantities are shown for mixtures with methanol and ethanol in Figs. 6.5 and 6.6. The broken horizontal axes in these figures serve the purposes of highlighting the lower and higher percentages and hiding the intermediate values, which were found to have negligible probability. As Fig. 6.4 (top) shows, the size of ionic clusters decreases when the amount of water in the mixture is increased, which is in good agreement with the results reported by Bernardes et al. [240]. Up to a water concentration around 90%, all the ions tend to be part of the same large cluster, which can in fact be identified as a polar IL network; after this percentage the probability of finding small ionic clusters starts to increase, and at over 98%of water most of the ions are isolated within bulk water. As expected, the behaviour of water molecules is exactly the opposite. As depicted in Fig. 6.4 (bottom), at 120 6.3. Results and discussion Figure 6.4 Probability of finding an ion (top) or a water molecule (bottom) in a cluster comprising a given percentage of the particles of that same type in the simulation box, for three different water concentrations. Solid circles mark the possible sizes: 𝑛=1,𝑛=2… starting from the left. The inset shows the probabilities for low concentrations in greater detail. 0 5 10 15 20 IL 0.0 0.2 0.4 0.6 0.8 1.0 25 % 80 % 99 % 0.0 0.2 0.4 0.6 0.8 1.0 95 96 97 98 99 100 solvent % of particles in the cluster 0.0 0.1 0.2 0.3 0.4 0.5 0.000 0.005 0.010 0.015 0.020 0.025 0.030 0.035 Figure 6.5 As in Fig. 6.4, but for methanol instead of water. 0 5 10 15 20 IL 0.0 0.2 0.4 0.6 0.8 1.0 25 % 80 % 99 % 0.0 0.2 0.4 0.6 0.8 1.0 95 96 97 98 99 100 solvent % of particles in the cluster 0.0 0.1 0.2 0.3 0.4 0.5 0.000 0.005 0.010 0.015 0.020 0.025 0.030 0.035 121 6. Nanostructure of imidazolium-based ionic liquids Figure 6.6 As in Fig. 6.4, but for ethanol instead of water. 0 5 10 15 20 IL 0.0 0.2 0.4 0.6 0.8 1.0 25 % 80 % 99 % 0.0 0.2 0.4 0.6 0.8 1.0 95 96 97 98 99 100 solvent % of particles in the cluster 0.0 0.1 0.2 0.3 0.4 0.5 0.000 0.005 0.010 0.015 0.020 0.025 0.030 0.035 low water concentrations isolated water molecules or those belonging to very small clusters (no more than 4or 5molecules) dominate the mixture. As the amount of water increases, the probability of finding water aggregates with larger sizes starts to rise, and over a water concentration of 85%many water molecules belong to a cluster whose size is very close to the total number of water molecules in the mixture, with only a few isolated or forming small independent water clusters. The fact that most water molecules are isolated at low water concentrations is consistent with conclusions previously reported in the literature [236, 239], and it has been attributed to the strong interaction between water molecules and anions [237, 243]. It must be noted that there is no particular tendency to the formation of ion pairs or larger uncharged clusters in preference to single ions or charged clusters. This may be attributed to the high dielectric constant of water, 𝜀􀂤􀂎􀂡􀂒􀂟 =78.5𝜀􀁭. As suggested by some previous results [222], the behaviour of clusters in IL + alcohol mixtures is markedly different. For IL + ethanol mixtures with 25% ethanol, Fig. 6.6 (top) shows that the size distribution of ionic clusters shares its main features with the case of IL+water mixtures. However, as more alcohol is added (for example, at 80%) the mode of the distribution is shifted from 100%to somewhat smaller percentages, which implies that the IL network has 122 6.3. Results and discussion been broken into large ionic clusters. This intermediate regime is not observed in mixtures with water at any concentration, since in that case ions predominantly appear either isolated or forming a single IL network. Figure 6.6 (top) also provides evidence of the tendency of ions to appear in pairs even at very high solvent concentrations, such as 99%ethanol. This is reflected in the fact that the mode of the distribution is not 𝑛=1, but 𝑛=2. Histograms for the most dilute IL + methanol mixtures (included as Fig. 6.5) reveal that, in contrast to this, within these systems isolated ions are more likely than ionic pairs. In regard to alcohol clusters, Figure 6.6 (bottom) shows that, although it is true that when more alcohol is present clusters somewhat larger than a dimer become possible, an alcohol network is never formed (even in pure alcohol), in stark contrasttowhat happensin water. This behaviour, now directly observed in the simulations, is probably at the root of the differences in equilibrium and dynamical properties of IL + water vs. IL + alcohol mixtures [222, 262]. Arguably, expressing concentrations in terms of mole fractions may not be the most informative choice as regards the spatial organisation of a liquid mixture. The ability of solvent molecules to interact among themselves depends not only on their number but also on the space available to them, related, in turn, to their molar volume. This is especially important when molecules of quite different sizes are being compared, as is the case in this work. Further insight can be gained by studying aggregation as a function of the volume fraction of solvent, 𝛷𝑠. By way of example, volume fraction is also considered the relevant magnitude for spatial occupation in the Flory-Huggins polymer solution theory [263] and the statistical lattice theory of mixtures [264], and will also be used in this role in Chapter 7. Figure 6.7 shows the same information asFig. 6.3butnowpresentedasa function of 𝛷𝑠. A setofequivalences between mole fractions and volume fractions are shown in Table 6.1. The densities used to build this table were also taken from GROMACS simulations, already proven capable of yielding reliable values of this variable [223]. The behaviour of ionic clusters is approximately universal when studied as a fraction ofsolvent volume fraction, due tothefact that, water moleculesbeing smaller than alcohol molecules, 𝛷􀂤􀂎􀂡􀂒􀂟(𝑥)is the slowest-growing function in Table 6.1, which neutralises the relatively small differences apparent in the left panels of Fig. 6.3. On the other hand, the greater tendency of water to form clusters is even more patent in Fig. 6.7: big clusters are clearly dominant in waterfromvolume fractionsas lowas20%, whereas for alcoholstheyare either totally absent (in ethanol) or present only at very high solvent volume fractions 123 6. Nanostructure of imidazolium-based ionic liquids Table 6.1 Volume fraction vs. mole fraction for the three solvents studied. 𝑥(%)𝛷􀂤􀂎􀂡􀂒􀂟 (%)𝛷􀂚􀂒􀂡􀂕􀂎􀂛􀂜􀂙 (%)𝛷􀂒􀂡􀂕􀂎􀂛􀂜􀂙 (%) 5 0.50 1.12 1.57 15 1.66 3.67 5.07 25 3.09 6.73 9.18 50 8.75 17.92 23.44 75 22.38 40.05 48.20 80 27.77 47.28 55.45 85 35.27 56.22 63.94 90 46.44 67.43 73.96 95 64.77 81.77 85.83 98 82.64 92.24 94.04 99 90.61 96.05 96.98 (in methanol). Even small solvent clusters, known from the detailed analysis of sizes performed above to be mainly aggregates of less than 10molecules, appear only very gradually when alcohol is added to the mixtures, while in water they contain nearly four out of ten solvent molecules at a solvent volume fraction just over 3%. Thus, from the analysis of cluster formation in mixtures of [BMIM][BF4] with water, ethanol and methanol it can be concluded that when a low amount of solvent is present in the mixture both water and alcohol molecules tend to be isolated from each other or forming clusters smaller than 4or 5molecules. When more solvent is added to the mixture, the probability of finding larger solvent clusters increases while at the same time the probability of finding all the ions in a single largecluster forming a polar network of IL decreases, which is a sign that solvent clusters are starting to break the ionic network. Finally, at very high water concentrationswater moleculestend to belong to a singlelarge clusterwhosesize is approximately thesameas thenumberofwater molecules present in the mixture, pointing to the formation of a water network that completely breaks the ionic network, since ions tend to be isolated or forming very small clusters at this water concentration. Figure 6.8 illustrates this by showing the ionic clusters at a particular time step for three water concentrations. Regarding alcohols, at very high concentrations ions tend to form pairs in mixtures with ethanol and to be isolated if the added solvent is methanol. This difference can be attributed to the lower dielectric constant of ethanol compared with water and methanol (𝜀􀂚􀂒􀂡􀂕􀂎􀂛􀂜􀂙 =33.0𝜀􀁭,𝜀􀂒􀂡􀂕􀂎􀂛􀂜􀂙 =24.2𝜀􀁭). Contrary to what happens in mixtures with water, far fewer, if any, very large clusters 124 6.3. Results and discussion Figure 6.7 As Fig. 6.3, but with the volume fraction as the independent variable. From top to bottom: water, methanol and ethanol. 0 20 40 60 80 100 In clusters In big clusters 0 20 40 60 80 100 0 20 40 60 80 100 0 20 40 60 80 100 0 20 40 60 80 100 % of ions Solvent volume fraction (%) % of solvent molecules of alcohol molecules are found at any amount of either ethanol or methanol, which suggests that alcohol molecules are homogeneously distributed in the structure of the imidazolium-based IL. This explains their reduced ability to break the IL network, reflected in the fact that an intermediate regime with large ionic clusters appears in mixtures with alcohol, but not in those with water. Another way to study the structure of mixtures of [BMIM][BF4] with water and alcohols is the analysis of the angular distribution of the solvent around the cation and the anion in the systems. To this end, a coordinate system centred on C2(the carbon atom between the nitrogen atoms in the ring) for the cation or B (the central boron atom) for the anion was taken, and the angle 𝜃􀁮between two vectors computed: the first is the position vector of the oxygen atom of the solvent; the second goes from the oxygen atom to the middle point of the two hydrogens (in water) or to middle point between the 𝐻and 𝐶atoms bonded to the oxygen (in alcohols). This definition is shown schematically in 125 6. Nanostructure of imidazolium-based ionic liquids Figure 6.8 Ionic clusters in a [BMIM][BF4] + water mixture with 25%(top), 95%(centre) and 99%(bottom) water. The different colours of the surfaces enclosing the clusters are intended to help differentiate them. The progressive breakdown of the ionic network can be observed. 126 6.3. Results and discussion Figure 6.9 Graphical scheme of the definition of 𝜃􀁮for two molecules, water and ethanol, around a [BMIM]+ion. The criterion for methanol is identical to that for ethanol. N N H O H OH Fig. 6.9 for water and ethanol; the definition for the latter of is also valid for methanol. Therefore, this second vector is parallel to the dipole moment of water, but forms an angle of 27.8∘with the dipole moment of ethanol and a 47.4∘angle with the dipole moment of methanol. The conditional probability density 𝑓(𝑐𝑜𝑠𝜃􀁮|𝑟),i.e., the probability density that a solvent molecule known to be placed at a distance 𝑟from a central ion is oriented in such a way that it yields a value of 𝑐𝑜𝑠𝜃􀁮in a particular interval, was then studied. This density provides a detailed picture of the structure of each solvation layer of both cations and anions. Figures 6.10 and 6.11 illustrate the probability density of 𝑐𝑜𝑠𝜃􀁮in [BMIM][BF4] + water mixtures for different distances and two water concentrations (25%and 95%, respectively) in order to analyse the orientation of the solvent around the cation (left) and the anion (right) and its evolution with the addition of solvent to the mixtures. Taking into account the definitions given above, in Figs. 6.10 and 6.11 it can be seen that those water molecules placed immediately beyond the vander Waals excluded volume of the ions are closely aligned with the monopole term of the cation and anion fields, since 𝑐𝑜𝑠𝜃􀁮=+1and 𝑐𝑜𝑠𝜃􀁮=−1, respectively. As expected from their charges, the cation prefers the region near the oxygen atom of water and far from the two hydrogen atoms, while the anion gets close to the oxygen atom approaching from between the two hydrogen atoms. Moreover, in the first solvation layer of water molecules around both the cation and the anion an exclusion area can be observed, antiparallel to the field, where no water molecules can be found. In the case of the solvation of the anion, at low water concentrations there is another exclusion area at around 0.5nmin which there are no water 127