scieee AI-readable full text Open interactive document viewer

Assessing the Effect of Surface Coating on the Stability, Degradation, Toxicity and Cell Endocytosis/Exocytosis of Upconverting Nanoparticles

Arellano, Lilia; Martínez, Raquel; Pardo Montero, Alberto; Díez, Iago; Velasco Rodríguez, Brenda; Moreda Piñeiro, Antonio; Bermejo Barrera, Pilar; Barbosa Fernández, Silvia; Taboada Antelo, Pablo

Abstract

Lanthanide-doped up-converting nanoparticles (UCNPs) have emerged as promising biomedical tools in recent years. Most research efforts were devoted to the synthesis of inorganic cores with the optimal physicochemical properties. However, the careful design of UCNPs with the adequate surface coating to optimize their biological performance still remains a significant challenge. Here, we propose the functionalization of UCNPs with four distinct types of surface coatings, which were compared in terms of the provided colloidal stability and resistance to degradation in different biological-relevant media, including commonly avoided analysis in acidic lysosomal-mimicking fluids. Moreover, the influence of the type of particle surface coating on cell cytotoxicity and endocytosis/exocytosis was also evaluated. The obtained results demonstrated that the functionalization of UCNPs with poly(isobutylene-alt-maleic anhydride) grafted with dodecylamine (PMA-g-dodecyl) constitutes an outstanding strategy for their subsequent biomedical application, whereas poly(ethylene glycol) (PEG) coating, although suitable for colloidal stability purposes, hinders extensive cell internalization. Conversely, surface coating with small ligand were found not to be suitable, leading to large degradation degrees of UCNPs. The analysis of particle’ behavior in different biological media and in vitro conditions here performed pretends to help researchers to improve the design and implementation of UCNPs as theranostic nanotools.

Full text

Journal of Colloid and Interface Science 668 (2024) 575–586 Available online 27 April 2024 0021-9797/© 2024 The Author(s). Published by Elsevier Inc. This is an open access article under the CC BY-NC license (http://creativecommons.org/licenses/bync/4.0/). Regular Article Assessing the Effect of Surface Coating on the Stability, Degradation, Toxicity and Cell Endocytosis/Exocytosis of Upconverting Nanoparticles Lilia Arellano a , 1 , Raquel Martínez a , 1 , 2 , * , Alberto Pardo a , * , Iago Diez a , 3 , Brenda Velasco a , Antonio Moreda-Pi˜ neiro b , Pilar Bermejo-Barrera b , Silvia Barbosa a , Pablo Taboada a a Colloids and Polymers Physics Group, Particle Physics Department, Materials Institute (iMATUS), and Health Research Institute (IDIS), University of Santiago de Compostela, 15782 Santiago de Compostela, Spain b Trace Element, Spectroscopy and Speciation Group (GETEE), Faculty of Chemistry and Materials Institute (iMATUS), University of Santiago de Compostela, 15782 Santiago de Compostela, Spain GRAPHICAL ABSTRACT ARTICLE INFO Keywords: Up-converting nanoparticles Surface coating Stability and degradation Endocytosis/exocytosis ABSTRACT Lanthanide-doped up-converting nanoparticles (UCNPs) have emerged as promising biomedical tools in recent years. Most research efforts were devoted to the synthesis of inorganic cores with the optimal physicochemical properties. However, the careful design of UCNPs with the adequate surface coating to optimize their biological performance still remains a significant challenge. Here, we propose the functionalization of UCNPs with four distinct types of surface coatings, which were compared in terms of the provided colloidal stability and resistance to degradation in different biological-relevant media, including commonly avoided analysis in acidic lysosomalmimicking fluids. Moreover, the influence of the type of particle surface coating on cell cytotoxicity and endocytosis/exocytosis was also evaluated. The obtained results demonstrated that the functionalization of UCNPs with poly(isobutylene-alt-maleic anhydride) grafted with dodecylamine (PMA-g-dodecyl) constitutes an outstanding strategy for their subsequent biomedical application, whereas poly(ethylene glycol) (PEG) coating, although suitable for colloidal stability purposes, hinders extensive cell internalization. Conversely, surface coating with small ligand were found not to be suitable, leading to large degradation degrees of UCNPs. The * Corresponding authors. E-mail addresses: [email protected] (R. Martínez), [email protected] (A. Pardo). 1 These authors contribute equally to this work. 2 Current address: Department of Physics, Clarendon Laboratory, University of Oxford, Parks Road, Oxford OX1 3PU, United Kingdom. 3 Current address: Department of Physics and Astronomy, Streatham Campus, University of Exeter, North Park Road, EX4 4QL, Exeter, United Kingdom. Contents lists available at ScienceDirect Journal of Colloid And Interface Science journal homepage: www.elsevier.com/locate/jcis https://doi.org/10.1016/j.jcis.2024.04.188 Received 15 September 2023; Received in revised form 26 March 2024; Accepted 26 April 2024 Journal of Colloid And Interface Science 668 (2024) 575–586 576 analysis of particle’ behavior in different biological media and in vitro conditions here performed pretends to help researchers to improve the design and implementation of UCNPs as theranostic nanotools. 1. Introduction Lanthanide-doped up-converting nanoparticles (UCNPs) have been intensively studied in recent years thanks to their ability to convert nearinfrared (NIR) excitation into ultraviolet (UV) and visible (Vis) emissions [1–3]. In the most typical design, UCNPs consist of NaYF 4 matrices doped with Yb 3+ ions as sensitizers that collect and transfer energy to codoped lanthanide ions (e.g. Er 3+ , Tm 3+ ) [4–6]. These activator ions provide intermediate metastable 4f excited states, which can generate effective up-converting luminescent emission upon sequential absorption of multiple low-energy photons into the energy levels of lanthanide dopants. Due to the long-lived intermediate energy states of lanthanide ions, UCNPs display enhanced properties compared to other luminescent materials, such as semiconductor quantum dots or organic dyes, in terms of luminescence lifetimes or resistance to photobleaching [7,8]. The intense tunable reemissions from UCNPs upon the absorption of NIR radiation allow deep and sharp tissue penetration, having been exploited in the biomedical field for detection [9], bioimaging [10], drug delivery [11], or photodynamic therapy [12]. Nevertheless, in view of the increasing use of UCNPs in biological applications, their potential dissemination, interactions with human cells/tissues, and potential harmful side effects must be considered in their design [13,14]. In this sense, it is worth mentioning the existence of several previous works that demonstrate the risks associated with the use/exposition of/to rare earth elements present in the structure of UCNPs [15–18]. In the specific case of nanoparticulated systems, the degradation of UCNPs involves important releases of F − , Y 3+ and Yb 3+ ions, giving rise to the presence of insoluble salts of lanthanide phosphates upon incubation in phosphate buffers [19]. To shield their interaction with the surrounding biological environment and avoid unwanted degradation while providing colloidal stability and biocompatibility, the surface chemistry of UCNPs appears as an essential factor [1,13,20]. Many different types of ligands and coatings have been proposed, ranging from small molecules and surfactants (e.g. ethylenediamine tetra(methylene phosphonic acid)) [16,21], to polymers (e.g. poly (ethylene glycol) (PEG)) [22–24], and inorganic coatings (e.g. silica) [24,25]. However, most commonly used coatings were unable to hinder the degradation of the UCNPs in biologically relevant media such as acidic lysosomal-mimicking fluids, thus varying their properties and compromising cell viability. Prompted by these findings, in this work we designed highly crystalline UCNPs and rendered them dispersible in biological media by means of different nanoparticle surface coatings. Besides evaluating a typical capping agent such as PEG, three other less explored coatings were analyzed: a polymer as poly(isobutylene-alt-maleic anhydride) modified by grafting with dodecylamine (PMA-g-dodecyl); and two small ligands such as meso-2,3-dimercaptosuccinic acid (DMSA) and 2- aminoethyl dihydrogen phosphate (AET). The evaluation of PMA-g- dodecyl was motivated by its proven excellent performance as coating in both magnetic and gold nanostructures [26–28], being its use with rare earth-based nanoparticles still very limited [29]. UCNPs functionalization with DMSA was analyzed despite its low suitability a priori owing to its small molecular size; nevertheless, in the basis of an own previous work, this coating rendered large ferrimagnetic nanostructures, which are prone to aggregate, highly stable in biological media [30]. Finally, AET coating was selected as an alternative low-molecular-weight ligand to establish a direct comparison with DMSA [29,31,32]. The influence of these nanoparticle coatings on the colloidal stability, degradation, biocompatibility, and cell endocytosis/exocytosis of UCNPs was exhaustively evaluated. 2. Experimental 2.1. Materials The detailed list of materials can be found in Supplementary Information. 2.2. Synthesis of UCNPs Highly-monodisperse cubic-shaped β-NaYF 4 :Yb 0.18 Er 0.02 UCNPs were obtained by mixing 1.60 mmol of YCl 3 ⋅6H 2 O, 0.36 mmol of YbCl 3 ⋅6H 2 O and 0.04 mmol of ErCl 3 ⋅6H 2 O with 33 mmol of oleic acid (OA) and 30.0 mL of 1-octadecene. The solution was heated to 150 ◦C and keep for 1 h under vacuum to eliminate oxygen and water traces. After cooling down to room temperature, 8 mmol of NH 4 F and 5 mmol of NaOH in 10 mL of methanol were added, forming a translucent yellowwhite solution after 30 min stirring at 50 ◦C. The methanol was evaporated by increasing the temperature to 80 ◦C under vacuum and, after 20 min, the solution became transparent. Then, the mixture was heated at 7 ◦C⋅min −1 up to 300 ◦C under N 2 atmosphere and kept at reflux for 1 h. The UCNPs were precipitated by adding methanol and centrifuging (2000 rcf, 10 min) and finally redispersed in chloroform [33,34]. The composition, size, and morphology of the UCNPs were tuned by modifying the ratios between lanthanide precursors and OA (see amounts of reagents used for the synthesis of each type of UCNPs in Supplementary Information: Table S1). 2.3. Aqueous phase transfer of UCNPs AET, DMSA and PEG functionalization: 20 mg of dried OA-capped UCNPs were dispersed in 5 mL of 1.0 mM HCl for 3 h. The remaining OA was extracted with 5 mL diethyl ether (three times). Next, the UCNPs were precipitated by adding acetone and centrifuging (1000 rcf, 15 min) and redispersed in 5 mL of AET, DMSA or PEG aqueous solutions (5 mg⋅mL −1 ) under sonication for 15 min. PMA functionalization: PMA was initially modified with dodecylamine (PMA-g-dodecyl) as reported elsewhere [35]. Then, 1 mL of OA-capped UCNPs at 5 mg⋅mL −1 was mixed with 1.5 mL of PMA-g-dodecyl at 0.25 M (monomer concentration), adding additional 5 mL of chloroform. The solvent was slowly evaporated in a rotavap and dried UCNPs were redispersed in 2 mL of 0.10 M sodium borate buffer (SBB) at pH 12. In all cases, the obtained UCNP@AET, UCNP@DMSA, UCNP@PEG or UCNP@PMA were collected by centrifugation (21000 rcf, 30 min) and washed three times to remove the excess of surface ligands. 2.4. Colloidal stability and degradation of UCNPs Spherical-shaped β-NaYF 4 :Yb 0.18 Er 0.02 UCNPs with the different surface coatings were dispersed in SBB, Dulbecco’s modified Eagles’s medium (DMEM), DMEM supplemented with 10 % (v/v) of fetal bovine serum (FBS), phagolysosomal mimicking medium (PSF), or PSF supplemented with 1 mM KF. The variations of ζ-potential and hydrodynamic size values were measured for 4 days. The degradation of UCNPs was evaluated by quantifying the released F − ions and the variation of luminescence emission intensity. For F − release studies, 1 mg⋅mL −1 of UCNPs were dispersed in the selected medium at 37 ◦C and incubated for the analyzed time. Afterwards, the UCNPs were collected by centrifugation (15000 rcf, 5 min), followed by ultrafiltration (MW 30 kDa) to eliminate any remaining particle. A potentiometric system with fluoride-ion-selective electrode (Methrom, Titrator Excellence T7) was used to quantify the amount of F − in the supernatants. Experimental L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 577 details about luminescence emission measurements can be found in Supplementary Information. The experiments were performed in triplicate. 2.5. Characterization Details of the characterization techniques can be found in Supplementary Information. 2.6. In vitro cell assays: Cytotoxicity and internalization of UCNPs Tumoral human cervical HeLa cells, murine Balb/3T3 fibroblasts and Raw 264.7 murine macrophages were purchased from Cell Biolabs (San Diego, CA, USA) and grown at standard culture conditions (5 % CO 2 at 37 ◦C) in DMEM supplemented with 10 % (v/v) FBS, 2 mM L-glutamine, 1 % (v/v) penicillin/streptomycin, 1 mM sodium pyruvate, and 0.1 mM nonessential amino acids. The in vitro cytotoxicity UCNPs was evaluated by means of the CCK-8 cytotoxicity assay. These cell viability data were complemented by measuring the cytokine release from macrophages, an indication of the inflammatory stress supported by cells which may lead to apoptosis. On the other hand, the uptake and internalization of UCNPs within HeLa cells was monitored by confocal microscopy. In addition, the influence of the UCNPs surface coating on cell internalization and clearance was also quantified by means of inductively coupled plasma mass spectrometry (ICP-MS). Experimental details of these procedures can be found in Supplementary Information. 3. Results and discussion 3.1. Synthesis and physical characterization of UCNPs In a typical synthetic procedure (see Experimental Section for details), monodisperse UCNPs were obtained through a bottom-up thermal decomposition method [36–38]. The morphology of the nanostructures can be controlled by varying the molar ratio between OA and lanthanide chlorides (Ln 3+ ) in precursor mixtures. In this way, we synthesized UCNPs based on NaYF 4 matrices doped with 18 % Yb 3+ and 2 % Er 3+ (NaYF 4 :Yb 0.18 :Er 0.02 ) displaying cubic, rod and spherical shape at OA: Ln 3+ molar ratios between 16.5 and 21.5 (Fig. 1A-D; Table S1 in Supplementary Information). Fig. 1. Transmission electron microscopy (TEM) images of NaYF 4 :Yb 0.18 :Er 0.02 UCNPs with: (A) cubic, (B-C) rod, and (D) spherical morphology prepared at OA:Ln 3+ molar ratio of 16.5, 19.0, 20.0 and 21.5, respectively. NaYF 4 :Yb 0.18 :Tm 0.005 UCNPs with (E) cubic, (F) mix rod/hexagonal, and (G-H) spherical morphology prepared at OA:Ln 3+ molar ratio of 16.5, 19.0, 20.0 and 21.5, respectively. (I) NaGdF 4 :Yb 0.18 :Er 0.02 nanospheres prepared at OA:Ln 3+ molar ratio of 19.0. Insets show statistical frequency (%) vs. size (nm) distributions (edge length for cubes, diameter for spheres and hexagons; length for rods; width distributions of rod-shaped UCNPs can be found in Fig. S1 in Supplementary Information). Scale bars 100 nm. L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 578 The different morphology of the designed UCNPs was attributed to the effect of the amount of OA chains incorporated in the synthetic process on the bottom-up growth mechanism of the particles. For a hexagonal NaYF 4 lattice (determined by X-ray diffraction (XRD), see below), the area of the {1010} facet exceeds that of the {0001}, so that the latter will have a higher surface energy and a faster growth rate. Thus, when the OA:Ln 3+ molar ratio is low, OA molecules would preferentially adsorb onto the {0001} facets, giving rise to nanocubes (Fig. 1A). With further increases in the OA:Ln 3+ molar ratio, the number of OA molecules reaches saturation on the {0001} facet and becomes progressively larger on the {1010} one, with larger surface area; in this manner, the growth velocity becomes progressively similar along the {0001} and {1010} directions, giving rise firstly to nanorods (Fig. 1B- 1C) and, then, to nanospheres when the velocity is equal in both facets (Fig. 1D) [39]. On the other hand, and despite the main focus of this work was to analyze the effect of the surface coating of UCNPs on their biological performance, we have also demonstrated the versatility of our strategy by synthesizing UCNPs with different compositions. Thus, the emission spectrum of the UCNPs was selectively tuned by incorporating Tm 3+ instead of Er 3+ as doping activator ions (NaYF 4 :Yb 0.18 :Tm 0.005 ). The substitution of 2 % Er 3+ by 0.5 % Tm 3+ slightly decreases the OA:Ln 3+ ratios at which the morphology transitions take place, being this attributed to the already established effect of lanthanide activator and extent of doping on the structure and physicochemical characteristics of the resulting UCNPs [40]. In this way, cubic-shaped, a mix of rods and hexagons and spherical-shaped UCNPs were obtained at OA:Ln 3+ ratios of 16.5, 19.0 and 20.0–21.5, respectively (Fig. 1E-H). Additionally, UCNPs composed of Gd 3+ instead of Y 3+ as constituent of the host matrices obtaining spherical-shaped NaGdF 4 :Yb 0.18 :Er 0.02 UCNPs at a Fig. 2. Structural and luminescence characterization of UCNPs. (A) EDX mapping analysis of spherical-shaped NaYF 4 :Yb 0.18 :Er 0.02 UCNPs (Scale bars 50 nm). (B) XRD patterns and (C) luminescence spectra upon 980 nm-laser excitation of cubic- (black) and spherical-shaped (green) NaYF 4 :Yb 0.18 :Er 0.02 , NaGdF 4 :Yb 0.18 :Er 0.02 (red), and NaYF4:Yb 0.18 :Tm 0.005 (purple) UCNPs. Photographs in (C) show the bare-eye emissions at different wavelengths of thulium- and erbium-doped UCNPs. L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 579 fixed OA:Ln 3+ molar ratio of 19.0 (Fig. 1I). However, as previously mentioned, these nanostructures were designed only as a proof of concept to demonstrate the versatility of our strategy to obtain UCNPs with different sizes, morphologies and/or compositions. An exhaustive study of their properties and applications will be the subject of a forthcoming publication. ICP-MS measurements confirmed the formation of the host matrices based on yttrium or gadolinium and the successful incorporation of the different sensitizer and activator ions within them according to the established precursor ratios (Additional File 1: Table S2). Moreover, energy-dispersive X-Ray (EDX) analysis was also performed for spherical-shaped NaYF 4 :Yb 0.18 :Er 0.02 UCNPs as example, confirming the presence of the different constitutive elements within the crystal matrices (Fig. 2A). On the other hand, XRD characterization showed that all the synthesized UCNPs display β-hexagonal crystal lattices, which agrees with their excellent luminescent emissions (Fig. 2B; see also Fig. S2 in Supplementary Information, where all the spectrums are represented). The presence of some minor residual peaks in XRD spectra (denoted with *) indicate the existence of small parts of particles’ structure with α -cubic crystallographic phase, while the peaks at ca. 32◦ arise from the presence of remaining OA chains. In terms of photoemission properties, NaYF 4 :Yb 0.18 :Er 0.02 UCNPs showed main emissions at 524 nm ( 2 H 11/2 → 4 I 15/2 ; green), 540 nm ( 4 S 3/2 → 4 I 15/2 ; green), and 654 nm ( 4 F 9/2 → 4 I 15/2 ; red) upon excitation with a non-collimated 980 nm laser beam. NaYF 4 :Yb 0.18 :Tm 0.005 UCNPs displayed emission bands at 360 nm ( 1 D 2 → 3 H 6 ; UV), 451 nm ( 1 D 2 → 3 F 4 ; violet), 476 nm ( 1 G 4 → 3 H 6 ; blue), and 840 nm ( 3 H 4 → 3 H 6 ; NIR), respectively, while NaGdF 4 : Yb 0.18 :Er 0.02 UCNPs showed similar emission lines as those of NaYF 4 : Yb 0.18 :Er 0.02 ones, as expected given their same activator element (Fig. 2C). 3.2. Surface modification of UCNPs For the intended biological applications of UCNPs, it is required to provide them with long-term colloidal stability in biological media while preventing their aggregation and/or degradation. For this purpose, we performed four different surface coatings of the designed UCNPs, taken spherical-shaped NaYF 4 :Yb 0.18 :Er 0.02 nanostructures as a model for their subsequent evaluation in various media of biological interest. The UCNPs with the different stabilizing agents were denoted as UCNP@AET, UCNP@DMSA, UCNP@PEG and UCNP@PMA. As expected, non-modified UCNPs with OA chains on their surface obtained by thermal decomposition were highly agglomerated when trying to disperse in water, displaying an average hydrodynamic size of 438 ±47 nm (Fig. 3A). After the functionalization processes, the successful attachment of the different ligands to the UCNPs surface was evaluated by Fourier-transform infrared spectroscopy (FTIR) (Fig. 3B; see the bonds associated with each band in Fig. S3 in Supplementary Information) [28,30,41–45]. Furthermore, the subtle changes observed in the particle surface charge also confirmed the successful attachment of the coating molecules to the UCNPs, displaying average ζ-potential values of −7.5 ±1.9 (UCNP@AET), –23.8 ±2.6 (UCNP@DMSA), −14.7 ±1.5 (UCNP@PEG), and –22.5 ±1.9 mV (UCNP@PMA). Thermogravimetric analysis (TGA) was performed to establish the weight percentage of the nanostructures attributed to the coating layers, observing that small ligands such as DMSA represent only ca. 12 % of weight of functionalized UCNPs while this percentage increases up to ca. 20 % in the case of larger polymeric structures such as PMA-g-dodecyl (Fig. S4 in Supplementary Information). Finally, dynamic light scattering (DLS) data showed that all the surface coatings provided the UCNPs with an initial high stability in water, displaying similar hydrodynamic sizes ranging from 104 to 110 nm (Fig. 3A). 3.3. Colloidal stability of UCNPs in biological media The colloidal stability of coated UCNPs was evaluated by monitoring their hydrodynamic size and ζ-potential upon 48 h incubation in two complex biological media: DMEM supplemented with 10 % (v/v) FBS and PSF. Thus, UCNP@AET displayed an initial hydrodynamic size of 106 ±8 nm in supplemented DMEM, which slightly increased within the first 12 h of incubation up to 122 ±6 nm, probably due to a combination of protein adsorption and certain particle destabilization caused by the high ionic strength of the medium. Further incubation led to remarkable particle size increasing up to 139 ±9 nm. In the case of UCNP@DMSA, the initial hydrodynamic size was 102 ±7 nm, displaying a starting ζ-potential of −13.3 ±0.7 mV. The hydrodynamic size was observed to slightly increase along incubation up to 117 ±5 nm, probably as consequence of the formation of a thin protein corona. No appreciable variation in their surface charges was noted except at 48 h of incubation, for which the ζ-potential slightly increased to −11.7 ±0.5 mV. For UCNP@PEG, the initial hydrodynamic size and ζ-potential values (101 ±8 nm and −13.4 ±1.0 mV, respectively) barely changed during the incubation time thanks to the steric hindrance provided by this polymer. The surface charge of UCNP@PEG was slightly negative as a consequence of the delocalization of electron pairs in the ether bond of PEG monomers, but contribution of some adsorbed protein molecules onto the particles’ surface cannot be completely neglected [46,63]. UCNP@PMA showed an initial hydrodynamic size of 106 ±9 nm and ζ-potential value of −14.3 ±1.8 mV, and both magnitudes barely varied during incubation time, which denoted an outstanding stability of UCNP@PMA in this medium (Fig. 3C). On the other hand, when the incubation was performed in PSF (see composition in Table S3 in Supplementary Information), important variations in the colloidal stability of the coated UCNPs were noted (Fig. 3D). UCNP@AET hydrodynamic sizes were observed to largely increased from the beginning of the incubation process up to 507 ±48 nm after 48 h, denoting a strong aggregation consequence of the experienced degradation, as shown later. UCNP@DMSA also underwent a remarkable increase on their hydrodynamic size during incubation from up 202 ±19 nm, with ζ-potential varying from −5.1 ±0.5 to −11.9 ± 1.8 mV. This denoted that DMSA coating provided better stability than AET, particularly at short incubation times, but both ligands are not suitable to achieve the desired protection of UCNPs in PSF. UCNP@PEG and UCNP@PMA showed high stability in acidic media, with hydrodynamic sizes within the range 110–125 nm during incubation and no signs of aggregation. On the other hand, progressive reductions in their surface potentials were observed up to −9.7 ±0.6 mV and −14.6 ±1.4 mV, respectively, thus providing certain electrostatic stability in addition to polymeric steric hindrance. (Fig. 3D). In summary, PEG and PMA-g-dodecyl coatings were able to provide UCNPs with high stability under some cell mimicking conditions, whereas DMSA and, especially, AET coatings become more unstable and were not able to hinder the aggregation of ceramic UCNPs. 3.4. UCNPs degradation In addition to the two media in which we previously assessed colloidal stability, the degradation study of UCNPs was expanded to other two simpler media: non-supplemented DMEM and SBB. Moreover, to analyze the effect of the presence of added F − ions on the degradation of UCNPs, we also studied PSF media supplemented with 1 mM KF. In this regard, it is worth mentioning that fluoride anions are essential in human body, being a micronutrient necessary to, for instance, prevent dental cavities and promote healthy bone growth [47,48]. As expected from previous studies [14,21], the designed UCNPs were low-degraded when dispersed in SBB medium, displaying reduced releases of F − ions and low decays on luminescence intensities even after 96 h incubation (Fig. 3E(i)-3F(i)). This low degradation degree was especially remarkable for UCNP@PMA and UCNP@PEG. A similar behavior was observed when the UCNPs were dispersed in nonsupplemented DMEM (Fig. 3E(ii)-3F(ii)). In the case of DMEM-FBS medium, UCNP@PMA and UCNP@PEG maintained a low degradation L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 580 Fig. 3. Colloidal stability and degradation of the UCNPs in biological media. (A) Population hydrodynamic diameter distributions and (B) FTIR spectra of sphericalshaped NaYF 4 :Yb 0.18 :Er 0.02 UCNPs coated with OA (black), AET (red), DMSA (blue), PEG (green), and PMA-g-dodecyl (magenta) dispersed in water after 0 h incubation at 37 ◦C. Colloidal stability of the functionalized UCNPs when: (C) incubated in DMEM +10 % (v/v) FBS analyzed in terms of (i) hydrodynamic size and (ii) ζ-potential variation; (D) incubated in PSF analyzed in terms of (i) hydrodynamic size and (ii) ζ-potential variation. (E) Fraction of F − released from NaYF 4 :Yb 0.18 : Er 0.02 UCNPs (X F ) upon incubation in (i) SBB, (ii) DMEM, (iii) DMEM +10 % (v/v) FBS, (iv) PSF, and (v) PFS +1 mM KF. (F) Luminescence decay ratio of NaYF 4 : Yb 0.18 :Er 0.02 UCNPs (L/L 0 ) upon incubation in (i) SBB, (ii) DMEM, (iii) DMEM +10 % (v/v) FBS, (iv) PSF, and (v) PFS +1 mM KF. UCNPs concentration was 10 μ g⋅mL −1 in all cases in (E) and (F). Polydispersity index associated with each DLS measurement can be found in Table S4 in Supplementary Information. L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 581 degree, but it increased markedly in the case of the particles coated with DMSA and, especially, AET (Fig. 3E(iii)-3F(iii)), being this fact attributed to the loss of stability derived from the larger adsorption of proteins on UCNPs’ surfaces. On the other hand, more important transformations of UCNPs occurred when incubated in PSF, observing large releases of F − ions and notable decays on luminescence signals, being these particularly stronger for UCNP@AET (Fig. 3E(iv)-3F(iv)). Interestingly, the presence of added F − ions in the PSF medium strongly decreased the degradation degree of the UCNPs (Fig. 3E(v)-3F(v)), in agreement with the fact that the maximum F − concentration is determined by its Fig. 4. Microscopy analysis of UCNPs degradation. TEM images of spherical-shaped NaYF 4 :Yb 0.18 :Er 0.02 UCNPs coated with AET, DMSA, PEG and PMA-g-dodecyl upon 0–48 h incubation in (A) DMEM +10 % FBS and (B) PSF. Scale bars 100 nm. L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 582 equilibrium value [19,49,50]. The observed relationship between the loss of luminescence and F − release from UCNPs is consistent with previous reports [19,51], being derived from the key role of particles crystallinity on the intensity of their luminescence emissions. However, luminescence signals can be also affected by flocculation of UCNPs or heterogeneous precipitation of other materials on the particles’ surface (e.g. phosphates in the case of PBS buffers) [52]. The effect of particle’s concentration was also briefly evaluated using UCNP@AET, observing larger degradation degrees in diluted dispersions (Fig. S5 in Supplementary Information). This fact might be considered when preparing dispersions with low circulating concentrations in the order of few tens/hundreds of μ g of UCNPs per mL, such as those typically used in biological applications [53]. TEM images were also acquired to evaluate the structural and physicochemical alterations of the diverse types of functionalized UCNPs when incubated in DMEM supplemented with FBS and PSF (Fig. 4). In the case of DMEM-based media, it was observed that the previously determined luminescence emission losses and large release of F − ions from UCNP@AET resulted in a low structural stability of the particles. UCNP@DMSA showed a remarkably lower degradation degree, being only noted some particle agglomeration. UCNP@PEG and UCNP@PMA maintained their well-defined morphology, in agreement with their lower release of F − ions to the medium, thus confirming the best protection against degradation provided by these coatings (Fig. 4A). Similarly, TEM analysis confirmed the important alteration of UCN- P@AET dispersed in PSF, with a partial loss of morphology and the formation of intertwined or agglomerated particle chains after 48 h of incubation. In the case of UCNP@DMSA, some particle surface alterations could be observed after incubation, being these variations more important than those previously observed when dispersed in DMEM- based medium. In the case of UCNP@PEG and UCNP@PMA, they again maintained high degrees of monodispersity upon 48 h incubation in PSF (Fig. 4B). In summary, we have demonstrated that PEG and, more especially, PMA-g-dodecyl coatings, provided UCNPs with high colloidal stability and resistance to degradation. In particular, PMA-g-dodecyl coatings preserved the luminescence intensities of UCNPs above 90 % and 80 % of original values after 96 h incubation in DMEM-based media and PSF, thus constituting a significantly higher protector against particles’ degradation than other previously proposed surface modifications [52,54]. The excellent performance of PMA-g-dodecyl coatings to render different nanostructured materials highly stable in aqueous media [26,28] is derived from the mechanism used to attach the polymeric molecules. In this sense, it was reported that surface coatings based on the deposition of additional amphiphilic layers, maintaining the original hydrophobic layers (i.e. polymer coating), gave rise to UCNPs with reduced non-radiative quenching by aqueous media in comparison with those that were rendered water-dispersible via ligand exchange processes [23]. We want to highlight that, unlike most previous works in which stability studies were very limited to PBS or DMEM-based media, the evaluation of the behavior of UCNPs in PSF here performed provided important information about the optimal coating of UCNPs. Thus, although the coatings with AET and DMSA rendered UCNPs with reasonably good protection when incubated in the most common media, their performance drastically dropped when they were evaluated in PSF. This fact limits the use of these surface modifications in applications that require the cellular internalization of UCNPs. To the best of our knowledge, the behavior of UCNPs in PSF media has hardly been analyzed before [16], being this stability/degradation study a valuable guide for the design nanostructures with cell internalization potential. 3.5. In vitro evaluation of UCNPs Thanks to their outstanding optical properties, UCNPs are being widely studied as potential nanotools for multimodal imaging and photodynamic therapy, amongst other applications. However, the potential harmful effects due to particle biotransformation or inherent component toxicity might preclude their translation to the clinics. To determine whether the UCNPs with the performed coatings are biocompatible, the viability of Balb/3T3 murine fibroblasts and human cancerous HeLa cells was assessed after 24–48 h of UCNPs administration by means of CCK-8 toxicity assays. As observed in Fig. 5A-C, all types of coated UCNPs were non-toxic for both cell lines after 24 h of incubation, with viabilities above 80 %. After 48 h, UCNPs showed a more remarkable concentration- and coating-dependent toxicity (Fig. 5B-D). Thus, cell viabilities larger than 80 % were only achieved at particles’ concentrations below 9.1 and 36 μ g⋅mL −1 when HeLa and Balb/3T3 cells were incubated in the presence of UCNP@AET. In particular, this kind of particles showed the lowest observed cell viability, reaching 41 % after 48 h of incubation in HeLa cells at the highest analyzed concentration (Fig. 5B). This behavior was attributed to the large release of F − ions from the structure of UCN- P@AET that can be harmful for cells, particularly for cancerous ones, which have a more accelerated metabolism. In the case of UCNP@DMSA, the critical concentration above which cell viabilities decreased below 80 % was 36 μ g⋅mL −1 in both cell types. For their part, UCNP@PEG and UCNP@PMA showed high cytocompatibility, with viabilities above 90 % for all the analyzed concentrations in both cell lines (Fig. 5A-D). The cytocompatibility of UCNPs was also evaluated by measuring the release of IL-6 and TNF- α cytokines from RAW 264.7 murine macrophages upon 24 h incubation. Although cytokine production is not directly related to cell mortality, it is a well-established indication of inflammatory stress supported by cells, which may lead to their apoptosis. The obtained results confirmed previous CCK-8 viability data, with UCNP@PMA and UCNP@PEG showing similar cytokines release than control cells. UCNP@DMSA and UCNP@AET reached much larger values, which confirm the high inflammatory stress induced by these typologies of particles in the cells, especially in the case of UCNP@AET at large concentrations. Bare UCNPs were also evaluated, observing cytokines release values up to six times those observed in control cells due to the low biological stability and the consequent high stress induced by these non-functionalized nanoparticles (Fig. S6 in Supplementary Information). Next, the internalization of UCNPs within HeLa cells was monitored through confocal microscopy. It is well-known that the quantum yield from upconversion in UCNPs is highly dependent on their surface chemistry, this being a factor that can distort the evaluation of the internalization of UCNPs with different coatings through the study of confocal microscopy images. However, the previously performed evaluation of their luminescence in biological media (Fig. 3F) allowed the use of emission intensity observed on confocal images to qualitatively compare the internalization degrees of the different particles. Thus, the internalization degrees of UCNP@PEG, UCNP@PMA and UCNP@DMSA in the first 24 h incubation can be directly compared based on the luminescence observed on the confocal images (similar emission profiles), while the strong decays on the luminescence of UCNP@AET must be considered on the analysis. Fig. 5E shows a strong luminescence inside the cytoplasm of HeLa cells along the first 6 h of incubation for UCNP@AET, which denotes a large cell uptake. The luminescence pattern indicates that the particles were aggregated within the cells, probably inside endo/lysosomes due to their lower pH, which would agree with colloidal stability data. However, after 24 h incubation the luminescence signals strongly decreased due to UCNPs degradation. The biological-induced removal of AET on the particle surface can be the origin of such degradation process since similar phosphate-based coatings have been demonstrated to be unable to protect the particles under abiotic and biotic conditions [16]. On the other hand, UCNP@DMSA and UCNP@PEG were also initially internalized within the cells, but at much lower extents than UCN- P@AET, due to the positive surface charge of these last ones in L. Arellano et al. Journal of Colloid And Interface Science 668 (2024) 575–586 583 comparison to the negatively charged cell membranes. For UCNP@DMSA, the luminescence signals from the particles were observed to progressively increase with incubation time and become more intense than for UCNP@AET after 24 h of incubation (Fig. 5E). This confirms the better protection of UCNPs provided by the DMSA coating compared to AET. Conversely, PEGylated nanostructures showed initially lower fluorescent signals within the cells, originated from the stealth properties of the PEG coating layer hindering interactions with cells and, thus, leading to lower uptakes. Nevertheless, once internalized, this type of UCNPs was well preserved within the cells, as denoted by the luminescence signals observed after 24 h of incubation. On the other hand, UCNP@PMA were initially internalized at similar degree than UCNP@DMSA, but they remain much more luminescently active inside the cells for longer times, corroborating the excellent protective role provided by this polymeric coating (Fig. 5E). The percentage of HeLa cells with internalized surface coated UCNPs after 6 and 24 h incubation was quantified from the obtained confocal microscopy images, corroborating the previously described observations (Fig. S7 in Supplementary Information). To confirm previous microscopy observations, the internalization of the different ligand-coated UCNPs inside HeLa cells was quantified by ICP-MS. Fig. 5F shows that the content of UCNP@AET inside cells was large and reached a maximum after 6 h of administration to subsequently decrease in agreement with confocal images. Conversely, internalized UCNP@DMSA reached a maximum inside cells after 24 h of administration to slightly decrease afterwards. A similar pattern was also observed for UCNP@PMA. Regarding UCNP@PEG, they were internalized at lower extents than the other types of UCNPs, which confirmed the stealthiness provided by PEG. Thus, we showed that, although AET coating promotes a rapid internalization of UCNPs within HeLa cells, the low protection provided caused faster degradation, agglomeration, and excretion of the particles. PMA-g-dodecyl and DMSA Fig. 5. Cell viability, endocytosis, and exocytosis of spherical-shaped NaYF 4 :Yb 0.18 :Er 0.02 UCNPs. Viability of HeLa cells after (A) 24 h and (B) 48 h, and Balb/3T3 cells after (C) 24 h and (D) 48 h of incubation with UCNPs. (E) Confocal images of HeLa cells after 6 h and 24 h incubation with UCNPs (Scale bars 10 µm). Quantification of UCNPs (F) endocytosed into HeLa cells and (G) exocytosed from HeLa cells after different incubation periods. L. Arellano et al.