scieee AI-readable full text Open interactive document viewer

Rigid biobased polycarbonates with good processability based on a spirocyclic diol derived from citric acid

Bonjour, Olivier,Liblikas, Ilme,Pehk, Tõnis,Khai-Nghi, Truong,Rissanen, Kari,Vares, Lauri,Jannasch, Patric

Full text

This is a self-archived version of an original article. This version may differ from the original in pagination and typographic details. Author(s): Title: Year: Version: Copyright: Rights: Rights url: Please cite the original version: CC BY-NC 4.0 https://creativecommons.org/licenses/by-nc/4.0/ Rigid biobased polycarbonates with good processability based on a spirocyclic diol derived from citric acid © 2020 The Royal Society of Chemistry Published version Bonjour, Olivier; Liblikas, Ilme; Pehk, Tõnis; Khai-Nghi, Truong; Rissanen, Kari; Vares, Lauri; Jannasch, Patric Bonjour, O., Liblikas, I., Pehk, T., Khai-Nghi, T., Rissanen, K., Vares, L., & Jannasch, P. (2020). Rigid biobased polycarbonates with good processability based on a spirocyclic diol derived from citric acid. Green Chemistry, 22(12), 3940-3951. https://doi.org/10.1039/d0gc00849d 2020 Green Chemistry PAPER Cite this: Green Chem., 2020, 22, 3940 Received 9th March 2020, Accepted 27th May 2020 DOI: 10.1039/d0gc00849d rsc.li/greenchem Rigid biobased polycarbonates with good processability based on a spirocyclic diol derived from citric acid† Olivier Bonjour, a Ilme Liblikas, b Tõnis Pehk, c Truong Khai-Nghi, d Kari Rissanen, d Lauri Vares* b and Patric Jannasch * a,b Introducing biobased polymers from renewable sources for use as high-performance thermoplastics with high demands on mechanical rigidity, transparency, thermal stability, as well as good processability, is a significant challenge. In the present work we have designed and prepared a rigid biobased bis-spirocylic diol by di-cycloketalization of a bicyclic diketone (cis-bicyclo[3.3.0]octane-3,7-dione, obtained from citric acid) using trimethylolpropane. This spiro-diol monomer has two reactive primary hydroxyl groups and the synthesis from inexpensive biobased starting materials is straightforward and readily upscalable, involving no chromatographic purification. In order to explore the usefulness of the new monomer, it was employed in melt polycondensations with diphenylcarbonate at up to 280 °C to form rigid fully amorphous polycarbonates (PCs). Molecular weights (MWs) up to M n = 28 kg mol −1 were achieved, and thermal and dynamic mechanical measurements showed glass transitions up to T g = 100 °C, with no thermal decomposition until T d ∼350 °C. Solvent cast films had excellent mechanical flexibility and strength, as well as a high transparency with only slight coloration. Results by dynamic melt rheology implied that the high-MW PCs had a good processability at 170 °C, with a stable shear modulus over time, but started to degrade via chain scission reactions when the temperature approached 200 °C. In conclusion, the present work demonstrates the straightforward preparation of the citric acid-based spiro-diol, and indicates that it is an efficient building block for the preparation of rigid biobased PCs and other condensation polymers. Introduction The development of sustainable biobased alternatives to fossilbased monomers and polymers has become increasingly important in recent years due to growing environmental, social and economic concern. 1,2 However, it is a considerable challenge to chemically design economically viable biobased polymers which meet all the strict requirements from highend applications on high-performance plastics with good processability. 3 For example, it is crucial that plastics intended for a wide range of automotive, construction, coating and packaging applications have a high degree of transparency and adequate thermal and mechanical properties to maintain dimensions and mechanical strength at elevated temperatures. This requires rigid polymers with a high glass transition temperature (T g ), high molecular weight (MW), as well as high thermal stability. Consequently, there is currently a need for biobased building blocks and monomers containing rigid aromatic and alicyclic rings to produce polymers with inflexible macromolecular chain structures. 3 Lignin is the most accessible source of rigid aromatic building blocks in the form of various phenolic compounds. 4 However, the depolymerization and purification of lignin is a complex and difficult process and so far vanillin is the only lignin-based compound that is commercially available. Despite these limitations, several high-T g lignin-based polymers 5 in the form of, e.g., polymethacrylates 6,7 and polyesters, 8–10 have been reported. When it comes to alicyclic monomers for polycondensation processes, isosorbide is probably the most studied and exploited alternative. 11 Isosorbide is a nonotoxic and chiral bicylic diol produced from sorbitol, which, in turn, †Electronic supplementary information (ESI) available. CCDC 1986990. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/ d0gc00849d a Department of Chemistry, Lund University, Box 124, Lund 221 00, Sweden. E-mail: [email protected] b Institute of Technology, University of Tartu, Nooruse 1, Tartu 50411, Estonia. E-mail: [email protected] c Laboratory of Chemical Physics, National Institute of Chemical Physics and Biophysics, Akadeemia tee 23, Tallinn 12618, Estonia d University of Jyvaskyla, Department of Chemistry, P.O. Box 35, Survontie 9 B, Jyväskylä 40014, Finland 3940 |Green Chem., 2020, 22,3940–3951 This journal is © The Royal Society of Chemistry 2020 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online View Journal | View Issue is a reduction product of glucose. 12,13 Despite the apparent benefits of incorporating isosorbide into polymers, the limited reactivity and stability are obvious drawbacks. 14 The low reactivity of the two non-equivalent secondary hydroxyl groups 15 impedes the formation of high MW polymers via polycondensation, and low MW polymers have insufficient mechanical properties. Increasing the polycondensation temperature (>230 °C) or reaction time to favor polymer chain growth typically leads to discoloration, cross-linking and degradation due to the limited stability towards thermooxidation. 14 Methods to improve the reactivity of isosorbide and other isohexides have been investigated and the strategies include the conversion of the secondary hydroxyl groups into primary ones via carbon chain extension, 16,17 and the development of more efficient catalyst systems. 18 Still, the intrinsic instability of the fused furan ring system needs attention. Gao, et al. have recently reported on octahydro-2,5-pentalenediol (OPD, Scheme 1), derived from citric acid. 19,20 Just like isosorbide, it has a rigid V-shaped structure, but instead of furan rings it has two cisfused carbocycles. This alicyclic diol yielded PCs with good thermal stability (thermal decomposition at 276 °C) and T g s up to 80 °C, demonstrating that the mimicking of the isosorbide bicyclic structure is an efficient approach to increase the chain rigidity of polymers. However, similarly to isosorbide, the secondary hydroxyl groups of OPD have low reactivity in polycondensation reactions and are likely to lead to low and medium MW polymers. The introduction of cyclic ketal and acetal units into polymers is a further attractive strategy to increase the T g and improve mechanical properties of polymers. 21 When an aldehyde or a ketone reacts with a suitable diol, a cyclic acetal or ketal, respectively, is formed. From this follows that the use of cylic ketones will lead to spiro-cyclic products, which are especially rigid. 21 The reactions proceed via acid catalyzed equilibria and the removal of water is necessary to reach high conversion. Acetals and ketals are typically stable towards bases but are susceptible to hydrolysis under acidic conditions. 22 Du Prez and coworkers prepared spirocyclic diol (“spiro-diol”) monomers in ketalization reactions of glycerol and two equivalents of 1,4-cyclohexanedione and 4,4′-dicyclo- hexanone, respectively. 23 Both monomers were successfully used to prepare PCs of high MW, but the synthesis of polyesters proved difficult and only low MW products were obtained. Recently, the biobased diketones camphorquinone and 1,4-cyclohexanedione were combined with glycerol to obtain stiffspiro-diols. 24 The corresponding PCs showed good mechanical properties, high thermal stability and high T g values. However, the isolation of these diol monomers required chromatographic purification, which makes them less attractive on larger scales. In another piece of work, Mankar et al. synthesized a spiro-diol by acetal formation in a reaction of pentaerythritol with two equivalents of vanillin. 25 Incorporation of this rigid spiro-cyclic diol in copolyesters produced from 1,6-hexanediol and dimethyl terephthalate resulted in improved T g and thermal stability. 25 Hence, this gave materials similar to Akestra™, a commercial fossil-based high-performance polyester produced from a spiro-diol, ethylene glycol and terephthalic acid. 26 Using a similar strategy, Warlin and coworkers reported the synthesis of a rigid spirodiol from pentaerythritol and two equivalents of fructosebased 5-hydroxymethylfurfural. 27 This monomer was employed to produce polyesters and poly(urethane-urea)s with increased T g s. However, the investigated spiro-diol was found to be heatsensitive, causing coloration and branching during the polyester synthesis. Besides the synthesis of various cyclic monomers, polycycloacetals and polycycloketals have been formed Scheme 1 Outline of the compounds based on diketone 1reported by McKeown and Gao, and in the present work (inside box). Spiro-diol 3 (mixture of cis and trans) was synthesized in a ketalization reaction of diketone 1and a slight excess of TMP 2(yields of 74 and 91% were obtained when the product was isolated by crystallization and chromatography, respectively). Green Chemistry Paper This journal is © The Royal Society of Chemistry 2020 Green Chem.,2020,22,3940–3951 | 3941 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online in direct polycondensations of tetraols and dialdehydes or diketones, respectively. 13 For example, McKeown et al. has reacted 1,5-diethylbicyclo[3.3.0]octane-3,7-dione with pentaerythritol in a polycondensation and achieved a spiro-polymer with a very high T g . 28 However, the degree of polymerization remained mediocre at ∼30, and the polymer was rather easily hydrolyzed in solution unless special precautions were taken (Scheme 1). In the present work we have designed and prepared a novel and readily accessible biobased tetracyclic aliphatic spiro-diol 3which combines the thermal stability of the rigid V-shaped alicyclic rings with the high reactivity of primary hydroxyl groups installed via the spiro rings (Scheme 1). The stiffbicyclic diketone cis-bicyclo[3.3.0]octane-3,7-dione 1was employed as a starting material. This diketone is derived via a Weiss–Cook condensation between glyoxal and dimethyl-1,3- acetonedicarboxylate (DAC). 29 Aqueous glyoxal can be prepared via oxidation of ethylene glycol. 30 A plant-based ethylene glycol production is currently under development by Avantium N.V. 31 DAC is readily derived from citric acid after decarboxylation and esterification. 32–34 Citric acid is an extensively used biobased platform chemical, produced via fermentation of glucose in more than 1.6 million tons annually. 35 Thus, the synthesis route of 1from citric acid is well-developed and involves only inexpensive acids (cat. H 2 SO 4 with H 2 O 2 or ClSO 3 H, aq. HCl, AcOH), base (NaOH) and MeOH. For the ketalization, we employed trimethylolpropane (TMP, 2), a triol widely used in the polymer industry that is available from Perstorp with partly renewable content (Evyron™). 36 The ketalization reaction between diketone 1and two equivalents of TMP 2then afforded the stiffspiro-diol 3, which bears two sixmembered spiro rings connected through a bicyclo[3.3.0] octane entity. Depending on the origin of the TMP (0, 20 or 50% renewable grade), spiro-diol 3has a 40, 50 or 70% content from renewable sources. Consequently, the overall synthesis route to spiro-diol 3is well-developed, readily up-scalable, and this monomer can be envisioned as a valuable biobased building block in various applications, including the preparation of different condensation polymers. In order to investigate the usefulness spiro-diol 3, we have in the present work studied the preparation of PCs in polycondensations with diphenylcarbonate, and subsequently investigated the thermal and mechanical properties, as well as the processability of the resulting materials. Results and discussion Monomer synthesis and structure elucidation A roughly 1 : 1 mixture of two isomers of spiro-diol 3was formed in the ketalization reaction of diketone 1with two equivalents of TMP 2in the presence of an acid catalyst in toluene/cyclohexane (Fig. 1a and Fig. S1–S6†). We speculated that these isomers are diastereomers that differ by mutual orientation of the terminal ethyl and hydroxymethyl groups (Scheme 1). The C 2 symmetric isomer was conveniently named as 3-trans and the C s symmetric as 3-cis. We separated these two isomers with the aim to unambiguously confirm the diastereomers. This separation turned out to be a routine task by standard flash chromatography on silica gel. The different symmetry of 3-trans and 3-cis is evident from their NMR spectra (Fig. 1 and Table S1†). In the bicyclo[3.3.0]octane subunit, the trans isomer has equivalent C-1 and C-5 and H-1 and H-5 chemical shifts, while the cis isomer shows different ones, separated in the 13 C and 1 H NMR spectra by 2.3 and 0.03 ppm, respectively. Further confirmation of the assignment of stereoisomers was obtained after single crystal X-ray analysis of the trans isomer. The single crystals of the compound 3-trans were obtained by slow evaporation of chloroform at ambient temperature. Fig. 2 presents the structure of 3-trans. In the solid-state the ethyl substituents of 3-trans are equatorial, while the hydroxymethyl groups are axial. The crystal lattice is stabilized via hydrogen bonds between the hydroxyl groups of 3-trans with its neighboring molecules. Crystal data, data collection and refinement details are given in the ESI.†Despite many attempts, no suitable single crystals from 3-cis could be obtained and thus its X-ray structure could not be determined. In the obtained conformation, the methylene carbons of the dioxane rings have both one trans and one gauche orientation to the bicycle methylene carbon atoms. However, from two bicycle methylene carbons, only one is having two gauche orientations. This is the main reason for the significant differences in the methylene carbon chemical shifts in the bicycle (7.4 in trans vs. 6.5 ppm in cis isomer) and the quite close values of the methylene carbon chemical shifts from the dioxane rings (for more comprehensive data, see Table S1†). During the course of the work we optimized the ketalization reaction, work-up and product isolation procedure to increase the efficiency for large scale synthesis of spiro-diol 3. In a preparative scale we chose to work with the diastereomeric mixture for practical reasons. This is also most relevant from an industrial point of view. We evaluated various solvents (mixtures of cyclohexane/DMF and cyclohexane/toluene, pure toluene), varied the stoichiometry of the reagents (1.95–3.5 eq. of TMP) and the amount of catalyst (1–20 mol% p-toluene- sulfonic acid, [p-TsOH]). The use of toluene as a reaction medium resulted in some darkening during the ketalization, probably due to the relatively high temperature needed for reflux. The lower boiling cyclohexane did not fully dissolve the starting materials. However, the addition of a small amount of DMF (10%) resulted in complete dissolution and a clean reaction. The removal of DMF is nevertheless tedious and its use is not recommended due to toxicity issues. 37 Finally, a 3 : 2 mixture of cyclohexane/toluene was identified as the best solvent system, affording a clean conversion without any noticeable by-product formation. The amount of acid catalyst had only a minor impact on the reaction outcome, and we found 1 mol% of p-TsOH to be a suitable concentration. An excess of TMP corresponding to 3.5 equiv. in relation to the diketone resulted in a somewhat faster ketalization reaction. Still, a smaller excess (2.2 equiv., i.e. 1.1 equiv. in relation to Paper Green Chemistry 3942 |Green Chem.,2020,22,3940–3951 This journal is © The Royal Society of Chemistry 2020 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online one carbonyl group) was enough to achieve a high conversion during 16 h. Detailed data from the optimization is presented in Table S2.† After cooling the reaction mixture and removal of the solvents by evaporation, three different work-up/product isolation methods were evaluated: (a) direct crystallization of 3in EtOAc/hex, 1 : 1, (b) dissolution of the directly crystallized product in EtOAc, washing with water/brine, followed by a second crystallization, and (c) flash chromatography. The direct crystallization (method a) afforded the crude product in Fig. 1 (a) 1 H spectrum of the mixture of 3-trans and 3-cis after isolation via double crystallization, and 13 C spectra of the (b) 3-cis and (c) 3-trans isomers after separation. Fig. 2 The X-ray structure of 3-trans (thermal displacement ellipsoids are shown at the 50% probability level). Green Chemistry Paper This journal is © The Royal Society of Chemistry 2020 Green Chem.,2020,22,3940–3951 | 3943 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online 85% yield. However, by careful analysis of 13 C NMR spectra, we detected a small amount of unreacted TMP present in the product. The aqueous wash (method b) removed the traces of TMP and the second crystallization afforded the pure product 3in 74% yield. Finally, the purification of the crude reaction mixture by flash chromatography (method c) afforded 3in 91% yield. Still, this method is less attractive from practical and economical points of view. The hydrolytic stability of spiro-diol 3in acidic environment was evaluated by using conditions reported by Liu and Thayumanavan 38 after modification: 1% aq. KH 2 PO 4 (pH = 4.5) in CD 3 CN at 20 and 60 °C, respectively, and 10 mM aq. trifluoroacetic acid (TFA) in CD 3 CN at 20 °C. The experiments were carried out directly in NMR tubes and monitored by recording 1 H NMR spectra at regular intervals. In the phosphate buffer at 20 °C, the diol was stable and no degradation was observed even after 7 days. However, after raising to 60 °C traces (<5%) of new signals that correspond to the partially hydrolyzed diol were observed after 24 h. In 10 mM aqueous TFA, the hydrolysis occurred faster. After 4 h at 20 °C roughly 50% of spiro-diol 3was left, and after 24 h all the diol had been cleanly converted into diketone 1and TMP 2(see Fig. S11†for 1 H NMR spectra at different time intervals). Polycarbonate preparation and structure characterization The diastereomeric mixture of spiro-diol 3was employed in the synthesis of PCs using diphenylcarbonate (DPC) as the carbonyl source (Scheme 2). Polymerizations were carried out as solvent-free melt polycondensations and we initially evaluated two different catalysts [NaHCO 3 , Li(Acac)], varied the ratio 3: DPC, and experimented with various heating/vacuum profiles (see Table S3†for detailed descriptions). A procedure adapted from Du Prez et al. was used as a starting point. 23 After this optimization to control MW and avoid degraded products, we prepared two PC samples using NaHCO 3 as catalyst and keeping the molar ratio of diol 3and DPC at 1.0 : 1.1. The MW of the first sample was purposely kept low and the second one high, to give the samples denoted PC-land PC-h, respectively (Scheme 2). In the preparation of PC-h, melt polycondensation temperatures up to 280 °C were applied, whereas for PC-lthe maximum temperature was limited to 210 °C. In the final stage when the temperature was raised to 280 °C, PC-h became highly viscous and started slowly to darken, after which the polymerization was terminated. In contrast, PC-l remained a viscous flowing melt throughout the polycondensation at 210 °C with no apparent color change. Both PC-land PC-hwere purified by precipitation in methanol from chloroform solutions. Further details on their synthesis are given in the Experimental section. Characterization by size-exclusion chromatography (SEC) using poly(ethylene oxide) standards showed M n = 7.5 and 27.7 kg mol −1 for PC-land PC-h, respectively (Table 1). As anticipated, PC-hreached a high MW, while that of PC-lwas significantly lower. Moreover, the analysis revealed polydispersities of Đ= 3.55 and 3.40, respectively. Under normal (ideal) conditions a value of Đclose to 2 is expected for polycondensations driven to high monomer conversions. 39 Hence, the higher values obtained in the present case may imply limited degradation via ring opening of the ketal rings during the polymerizations, which would result in branching and a broadening of the chain length distribution. This was also hinted by the shape of the SEC curves, which show high-MW shoulders (Fig. S12†). Similar findings have previously been reported by Du Prez et al. who found Đin the range 2.8–3.2 for PCs(M n = 24–33 kg mol −1 ) prepared by melt polycondensation of DPC and ketal diol monomers. 23 For polyesters based on the same ketal monomers, the range in Đwas 2.3–4.0. In addition, Suh and coworkers synthesized a PC by polycondensation of DPC and the bis(glycerol) ketal of camphorquinone, and reported Đ= 2.25 (M n = 8.3 kg mol −1 ). 24 Characterization by 1 H and 13 C NMR spectroscopy confirmed the structure of the PCs (see Fig. 3 and Fig. S7 and S8†). Detailed analysis of the spectra of PC-hindicated that the cis and trans isomers of 3preserved the shift differences. The carbonyl region at 155 ppm revealed the dyad level sequences of the polymer, showing clearly the presence of cis–cis, Scheme 2 Synthesis of PCs by melt polycondensations of diol 3with DPC using the mixture of the 3-trans and 3-cis isomers. Table 1 Data on the PCs based on diol 3 Sample Isolated yield (%) M n (SEC) (kg mol −1 )Đ(SEC) M n (NMR) (kg mol −1 )T g (DSC) (°C) T g (DMA) (°C) T d,95 (TGA) (°C) PC-l86 7.5 3.55 7 85 85 352 PC-h90 27.7 3.40 22 100 99 360 Paper Green Chemistry 3944 |Green Chem.,2020,22,3940–3951 This journal is © The Royal Society of Chemistry 2020 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online cis–trans and trans–trans dyads in roughly 1 : 2 : 1 ratios (Fig. 3). This indicates that the reactivity of each hydroxyl group is independent, and is hence not influenced by the relative orientation of the other hydroxyl group in diol 3. Close inspection of the 1 Hand 13 C NMR spectra also indicated the complete lack of any aromatic signals potentially originating from DPC residues at the chain ends. On the other hand, small signals from terminal –CH 2 OH groups were clearly present at 62.7 ppm in the 13 C NMR spectra (Fig. S9 and S10†). Assuming linear chains with exclusively –CH 2 OH end groups, the intensity of these signals in the spectra of both PC-land PC-hwere in level with that expected from their respective degree of polymerization measured by SEC. Hence, the end group analysis based on the signals from terminal –CH 2 OH groups indicated M n = 7.0 and 22 kg mol −1 for PC-land PC-h, respectively. The slightly lower values obtained in the end group analysis may indicate limited branching, which is in agreement with the finding that Đ> 2. Still, we cannot rule out that the observed differences in the M n values are explained simply because SEC analysis using poly(ethylene oxide) standards and calculations based on small NMR signals give different results. After drying, the precipitates of both PC-land PC-hwere completely soluble in CHCl 3 and THF, partially soluble in 1,4- dioxane, EtOAc and toluene, and insoluble in water, MeOH, iPrOH, acetone, hexanes, diethyl ether and CH 3 CN. The PC-h precipitate had a “cotton-like”appearance with clearly visible fibers, reflecting its high MW, while the PC-lprecipitate was a fine powder as expected from its low MW. Both PC samples were cast from solution to study their ability to form films. The PC-hfilms were only slightly colored (Fig. 4) with high transparency (Fig. S13†) and gloss (between 75 and 118 gloss units [GU]), combined with an excellent mechanical flexibility (ESI Movie†) and strength (Fig. S14†). The films formed by PC-lwere less colored, equally transparent, but showed brittleness due to the lower MW. Thermal characterization The T g and the thermal decomposition temperature (T d,95 )of the PCs were evaluated by DSC and TGA measurements, respectively. At the T g the polymer starts to soften and lose its mechanical rigidity, and hence this value normally sets the upper use temperature in a given application. As seen in Fig. 3 (a) 1 H and (b) 13 C spectra of PC-h. 13 C signals indicating the 1 : 2 : 1 ratios of cis–cis,cis–trans and trans–trans dyads are shown separately in the carbonyl region. Green Chemistry Paper This journal is © The Royal Society of Chemistry 2020 Green Chem.,2020,22,3940–3951 | 3945 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online Fig. 5a, PC-hshowed T g = 100 °C, which is in range with polystyrene. 40 As expected, the DSC traces did not show any crystallization or melt transitions. Hence, PC-his a fully amorphous polymer that will retain mechanical rigidity at temperatures approaching 100 °C. Poly(trimethylene carbonate) and poly (propylene carbonate) have T g values at approximately −17 °C 41 and 30 °C, 42 respectively, which demonstrates that the incorporation of the tetracyclic spiro-diol 3has the potential to significantly increase the T g of aliphatic PCs. The high T g of PC-hmay open up for, e.g.,“hot-fill”applications in food packaging and handling. The value may further be compared to the semicrystalline PET (T g = 75 °C), 43 as well as with PC based on bisphenol A (T g ∼150 °C), 44 and the Akestra™family of polyesters (T g in the range 90–110 °C, depending on monomer content). 26 The DSC analysis of PC-lshowed a T g value of 85 °C, i.e., 15 °C below that of PC-h. This was anticipated because of the significantly lower M n value of the former polymer (7.5 vs. 27.7 kg mol −1 ). The lower T g and M w values suggest potential applications as, e.g., specialty polyols in the preparation of polyurethanes. The T d,95 value measured by TGA analysis typically determines the maximum melt processing temperature of a polymer. Both PC-hand -lshow thermal decomposition in a single step at T d,95 ∼350 °C (Fig. 5b). This indicated that the thermal stability of these materials is sufficiently high to allow melt processing which (depending on method, MW, etc.)is typically performed ca.50–100 °C above T g . In order to study the long-term stability, isothermal TGA measurements were carried out at 170 and 200 °C, respectively, during 8 h with the samples in the melt state. As seen in Fig. 6, the two PC samples showed different behavior under these conditions. At 170 °C, PC-lshowed an initial weight loss of just above 2 wt%, before reaching a plateau. At 200 °C the initial weight loss had the same magnitude, but was followed by a constant weight loss (decomposition) rate of ∼0.30 wt% per h. The initial weight loss may be due to the presence residual solvent or monomer. For PC-h, the weight slowly increased by ∼0.8 wt% and then seemed to reach a plateau value. This increase was most probably due to limited oxidation of the sample. In contrast, the same sample displayed a steady weight loss rate of ∼0.15 wt% per h at 200 °C, i.e., half that of PC-l. Dynamic mechanical characterization The dynamic mechanical properties of the PCs were studied by DMA analysis of hot-pressed sample bars at 1 Hz in the linear viscoelastic region (tensile strain 0.02%). Fig. 7 shows the tensile storage (E′) and loss (E″) moduli of the two PC samples during heating at a rate of 2 °C min −1 . As can be seen, the E′ value on the glassy plateau was higher for PC-hbecause of its higher M n value compared to PC-l. Consequently, PC-hhad an Fig. 4 Photograph of a 45 μm thick film of PC-hcast from CHCl 3 solution. Fig. 5 DSC (a) and TGA (b) traces of PC-hand -l, respectively. Fig. 6 Isothermal TGA measurements of PC-land -hat 170 and 200 °C. Paper Green Chemistry 3946 |Green Chem.,2020,22,3940–3951 This journal is © The Royal Society of Chemistry 2020 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online E′value of 0.90 GPa at 90 °C, while PC-lhad an E′value of 0.42 GPa at 60 °C. The decrease in E′marked the start of the glass transitions of the two PCs. Notably, the transition occurred in a broader temperature range for PC-lthan for PC-h, which may be a consequence of the broader Đvalue and hence larger heterogeneity of the former sample. After the transition region, i.e., just before entering the rubbery plateau, the samples deformed too much to continue the measurements. The T g was indicated by the maximum in E″and showed T g = 85 and 100 °C for PC-land PC-h, respectively. These values were essentially the same as those evaluated by DSC, which demonstrated a very good correlation between the two methods. Dynamic melt rheology Dynamic rheology measurements were primarily carried out to assess the stability and processability of the PCs in the melt state. Rheological properties are related to MW and structure, and changes in the modulus may thus indicate degradation by, e.g., polymer chain scission or crosslinking reactions. 45 The data of the present polymers was measured by using hotpressed sample discs in a parallel plate arrangement. Time sweeps were carried out during 20 min at a frequency of 1 Hz at 0.2% strain, which was within the linear viscoelastic region. Fig. 8a shows the melt shear storage modulus (G′) and phase shift (δ)ofPC-has a function of time at 170 and 200 °C, respectively. As can be seen, the data at 170 °C were constant over time with G′and δequal to 42 kPa and 43°, respectively. This indicated a high stability of the sample without apparent signs of any polymer chain degradation. Initially, the measurement at 200 °C showed a decrease in G′and an increase in δ, in relation to the data at 170 °C. This was consistent with the expected decrease in viscosity and less elastic response of the melt as T−T g increased. In sharp contrast to the data at 170 °C, there was a clear decrease in G′and a corresponding increase in δobserved over time at 200 °C. These changes towards a less elastic material are consistent with a reduction in MW over time. Hence, the data in Fig. 8a implies that PC-h is processable in the melt at 170 °C, but starts to degrade by chain scission reactions when the temperature approaches 200 °C. Fig. 8b shows the corresponding values of G′and δof PC-l as a function of time at 170 °C. Compared to the data of PC-h, the initially measured value of G′was lower and the δvalue higher. This was consistent with the lower MW of PC-l, resulting in a less elastic response. Over time, the data of PC-l showed a clear increase in G′and a corresponding decrease in δ. These trends towards a more elastic material are consist- Fig. 7 Tensile storage (E’) and loss (E’’) moduli of PC-land -h,as measured by DMA at 1 Hz, 0.02% strain. Fig. 8 Variation of the melt shear storage modulus (G’) and phase shift (δ) during time sweeps of PC-hat 170 and 200 °C (a) and PC-lat 170 °C (b), as measured by rheology at 1 Hz, 0.2% strain (note the different scales for G’). Green Chemistry Paper This journal is © The Royal Society of Chemistry 2020 Green Chem.,2020,22,3940–3951 | 3947 Open Access Article. Published on 28 May 2020. Downloaded on 7/17/2020 1:37:12 PM. This article is licensed under a Creative Commons Attribution-NonCommercial 3.0 Unported Licence. View Article Online