scieee AI-readable full text Open interactive document viewer

Chemical, mineralogical and physical study of Late Iron Age ceramics from Nditam: Cameroon (West central Africa)

Epossi Ntah, Zoila Luz,Cultrone, Giuseppe V.

Abstract

Junta de Andalucía Research Group RNM179

Full text

ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 https://doi.org/10.1186/s40494-023-01120-1 RESEARCH Chemical, mineralogical andphysical study ofLate Iron Age ceramics fromNditam: Cameroon (West central Africa) Epossi Ntah Zoila Luz1* and Cultrone Giuseppe2 Abstract This paper studied Late Iron Age ceramic fragments from Nditam village (Centre Region, Cameroon), the technological features and deduced the type of the raw materials used to produce them by combining different analytical techniques based on X-ray fluorescence, powder X-ray diffraction, thermogravimetry, polarized optical microscopy, spectrophotometry and hydric tests. Macroscopic observations suggest the existence of three types of ceramics according to their colour, black, greyish and red, in the two opposite surfaces, outer (or external) and inner (internal). The chemistry indicates that non-calcareous clayey material was used for ceramic production. The correlation between mineralogy, petrography and the geology of the region suggests a local production of ceramics. Moreover, the chemistry of the samples confirms the existence of the three macroscopic groups and suggests the use of local raw materials for their production. From the mineralogical point of view, quartz, feldspar and mica (biotite and muscovite) were identified in all the samples, while kaolinite and amphibole were detected in some of them. The differences in the mineralogy may indicate some variations in the firing temperature, being lower in the ceramics containing kaolinite compared to the other samples. All the samples have similar water absorption behaviour. According to the colours of the ceramics, a prevalence of oxidising firing conditions was present in the kilns. However, partial reducing and short duration firing conditions were also possible. Comparative study with the mineralogy of ethnographic ceramics from southern Cameroon shows some similarities and suggests a continuity in the use of different local clay pits in this region over time. Keywords Nditam/Cameroon, Ceramics, Petrophysical characterization, Firing technology, Raw material Introduction andarchaeological background Any ceramic fragment, however insignificant it may appear, can be compared to a ’’potential book’’ because it contains as if stored in pages, a wealth of information about its history [1]. Its memory can be activated by a variety of chemical, mineralogical and physical analyses in order to shed light its origin, manufacture, use and burial stage. It should be noted that the technological choices of the potters were always linked to natural resources, the cultural traditions of their community and its natural background. Therefore, the choices of raw materials, ceramic fabrics and recipes, firing conditions and ways of forming vessels are linked to the local environment as much as to the abilities and experience of the potters [2]. In central Cameroon, sixty archaeological sites were discovered during an archaeological excavation in the Tikar area from 1993 to 1997 [3, 4]. These sites were open-air, metallurgical (workshops of iron and bronze production) and rock shelters. The second main excavations in the Tikar area were conducted between Open Access © The Author(s) 2023. Open Access This article is licensed under a Creative Commons Attribution 4.0 International License, which permits use, sharing, adaptation, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if changes were made. The images or other third party material in this article are included in the article’s Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http:// creat iveco mmons. org/ licen ses/ by/4. 0/. The Creative Commons Public Domain Dedication waiver (http:// creat iveco mmons. org/ publi cdoma in/ zero/1. 0/) applies to the data made available in this article, unless otherwise stated in a credit line to the data. Heritage Science *Correspondence: Epossi Ntah Zoila Luz [email protected]; z[email protected] 1 Department of Arts and Archaeology, Faculty of Arts, Letters and Social Sciences, University of Yaounde 1, P.O.Box 755, Yaounde, Cameroon 2 Department of Mineralogy and Petrology, Faculty of Sciences, University of Granada, Avenida Fuentenueva, s/n18002, Granada, Spain Page 2 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 2005 and 2013 in four sites: Nditam, Ngoumé, Gba and Ngweu [5] (Fig.1a). The ceramics selected for the present study come from Nditam (5°00′18″ N and 11°50′31″), a village located in the southern part of the Tikar Area and about 250 km far from of Yaounde in the Centre Region of Cameroon. The region is a forest—savannah transition (Fig.1b). In Nditam, many pit sites were discovered. Delneuf and Tueche [3] identified a long chronological sequence made up of three main periods. The Nditam phase 1 started from 1319 to 896 BC and was characterized by the presence of the first pit sites, lithic fragments (shards/flakes of quartz) and ceramics with pivoting impression decoration. Nditam phase 2 had two stages, 540–349 BC and 321–206 BC, which were characterized by the beginning of iron metallurgy, the abundance of pits, ceramics with pivoting impressions and lithic materials (stone ball). The Nditam phase 3, the most recent, started from 1487– 1603 AD and was characterized by the beginning of the ceramics with roulette decoration patterns and by the continuity of iron metallurgy. The gap between phases 2 and 3 is explained by the absence of data, therefore more excavations and radiocarbon dating are still needed in this region. Morphological, decorative and stylistic aspects of the ceramics from Nditam have already been studied by Leka [5]. Roulette, comb and fiber impressions were abundant in the most recent ceramics whereas pivoting impressions and incisions were found in the most ancient ones. Morphologically, these ceramics can be classified into flared and narrowed ware characterized by spherical, hemispherical, sub-hemispherical, ellipsoidal, sub-cylin- drical and truncated-cone shapes according to the large variety of rim, body and base fragments studied. A preliminary characterization of the non-plastic inclusions and colour of 5706 ceramic fragments from Nditam was performed by the naked eye and stereomicroscopic observations showing fine to semi-fine pastes with different colours, grey, brown, red and beige [5]. These colours suggest a variety of firing conditions. The non-plastic inclusions were composed of quartz, feldspar, micas, iron nodules, laterite fragments and organic matter imprints. These inclusions were medium to poorly sorted with sizes ranging from 0.5 to 4mm. Leka [5] suggested the use of a mixture of clays or the addition of sand to the clay to improve the quality of the paste. The study of the provenance of the ceramics was not carried out. The present paper will centre on selected ceramics belonging to the Nditam phase 3 (1487–1603 AD) to understand the nature of the raw material used in ceramics production and the technology process (clayey material preparation, addition or not of temper and firing conditions) in order to provide those archaeometric data that can help improve and complete the knowledge of ceramic production techniques in Nditam. Although the Nditam area has not yet been examined from the Fig. 1 a Archaeological sites found in the Tikar area; b location map of the Tikar area in Cameroon from Leka [5] Page 3 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 archaeometric point of view for the study of ceramics, other research has been carried out in the central part of Cameroon, in particular at Mfomakap [6]. Archaeological ceramics from Mfomakap (1905 ± 25 BP) corresponding to the Early Iron Age were characterized by the combined use of chemical, mineralogical and textural techniques with the aim of determining their technology and provenance. For this purpose, local raw materials and ceramic fragments were analysed and compared. In that case, a local production of ceramic products was suggested. In the same line, a mineralogical study of ethnographic ceramics from Bankim, another locality in the Tikar plain was conducted in order to determine the evolution of temperature at different during pre-firing and firing process [7]. The correlation between the analytical techniques suggested that the pre-firing temperature was below 450 °C whereas the firing temperature was between 650–800℃ in a simple bonfire. The present work aims to enhance the contribution of analytical methods in the study of archaeological ceramics from Cameroon as a database for future studies. In this respect, X-ray Fluorescence will help answer questions about the nature and origin of the raw material used by the potters [8, 9]. X-ray diffraction and thermogravimetric analysis (TG) will be used to identify the mineral phases and inform about the firing temperature whereas the firing atmosphere will be deduced from the macroscopic observations of the ceramics, mainly the colour of the fracture surface [10, 11]. Polarized optical microscopy will be used to analyse the fabric of ceramics to determine the nature of the inclusions present in the paste, clay preparation and nature of temper. Finally, spectrophotometry and hydric tests (water absorption and drying) will complete the characterization of ceramics providing some physical parameter (colour and water flow in the porous system) that will help in defining their quality [12, 13]. These results will give an idea of the technological level of the local potters and to their skills to use natural resources [2]. Geology ofthearea The Tikar plain, situated in the Cameroon Central Shear Zone, is part of the North Equatorial Pan-African Belt. It is formed by granitoids rocks intruded sometimes by mafic and intermediate dykes [14]. The mafic dykes are essentially banded gabbro with porphyroblastic to porphyritic textures and are composed of plagioclases, pyroxenes, amphiboles, biotite and opaque minerals. The intermediate dykes are monzonites and monzodiorites characterized, respectively, by cataclastic and mylonitic textures [15] and composed of amphiboles, K-feldspar, pyroxenes, epidotes, titanite and opaque minerals. The above-mentioned magmatic rocks are covered in the Tikar plain by clays and sands from the Quaternary age [16]. It is logical to assume that these sediments were used by potters for ceramic production. A schematic geological map of the Tikar plain is presented in Fig.2. Materials andmethods Samples Thirteen ceramic samples of the Late Iron Age (1487– 1603 AD) were selected from the collection of the Department of Arts and Archaeology of the University of Yaounde 1 (Cameroon) to be studied in the present paper. All the selected ceramics are shown in Fig.3. They were labelled CNDI 01 to CNDI 13. They show fine to semi fine surfaces and appear macroscopically different on the ornament, colour (external, internal and fracture surface), size and shape. They belong to the rim and body parts of vessels. Except CNDI 08, all the other samples are decorated. The ornaments observed on the surface are simple line bands due to tracing and/or incision (CNDI 01, CNDI 03, CNDI 04 and CNDI10), impression (CNDI 01, CNDI 02, CNDI 07, CNDI12 and CNDI13) and roulette (CNDI 04, CNDI 05, CNDI 09 and CNDI 11). The thirteen samples were classified in three groups according to their external and internal surface colours: Group 1 is characterized by a black colour: one sample (CNDI 05). Group 2 is characterized by a greyish colour (light or dark grey): eight samples (CNDI 03, CNDI 04, CNDI 07, CNDI 08, CNDI 10, CNDI 11, CNDI 12 and CNDI 13). Group 3 is characterized by a reddish colour (dark or light brown): four samples (CNDI 01, CNDI 02, CNDI 06 and CNDI 09). CNDI 06 and CNDI 01 show some dark areas on their external surface probably due to their use. Only one sample, CNDI 06, shows a sandwich structure (with a black core), while the rest have brown or reddish fracture surfaces and one sherd, CNDI 04, has a totally dark grey fracture surface. A summary of the main features of the thirteen ceramics is listed in Table1 and the representative ceramics for the three groups are presented in Fig.4. Analytical methods The chemical composition of ceramics was determined by X-ray Fluorescence (XRF) analysis using a Panalytical Zetium spectrometer equipped with a Rh tube anode and 4 kV X-ray generator. For major elements, a mixture of 0.6 g of powdered sample with 5.4 g of Li2B4O7 was melted at 1000 °C; after cooling the disc glass was analysed. For trace elements, a mixture of 5 g of sample in the same proportion with boric acid was pressed to produce a pellet for analyses. The accuracy of the chemical analyses was assessed by comparison with more than 30 Page 4 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 certified geostandards covering a wide range of common silicate rocks [17] and XRF intensities were converted to concentrations using the De Jongh model [18]. Typical accuracy is better than 0.1–0.2% relative (0.5% for Na2O) to a concentration of 10%. Loss on ignition was determined gravimetrically by recording weight loss between 110 ℃ and 1000 ℃. For trace elements, the detection limit is below 1–2 ppm, except for Ba and Co, which are around 10–15 ppm. Powder X-ray Diffraction (PXRD) analysis was carried out by using a Bruker D8-Advance Eco 1 Kw diffractometer (CuKα radiation, λ = 1.5418 Å, V = 40 kV, I = 25 mA) with a Lynx-eyed X energy-dispersive detector. PXRD patterns were recorded over the 2 -70° (2θ) angular range. Fig. 2 Schematic geological map of Tikar Plain Page 5 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 Fig. 3 General view of the thirteen ceramic samples from their external surface (size of the square edge: 1 cm) Table 1 Macroscopic features of the studied ceramic samples The division into three groups is based on ceramics internal and external surface colours Samples Group Ornament Part of the vessel Type of ware Colours External surface Internal surface Fracture surface CNDI 01 3 Impression Rim Semi fine Dark red Reddish Reddish CNDI 02 3 Impression Body Semi fine Dark red Light brown Light brown/ reddish CNDI 03 2 Tracing/ incision Rim Fine Dark greyish Grey Reddish CNDI 04 2 Carved roulette + tracing Rim Fine Light grey Grey Dark grey CNDI 05 1 Carved roulette Rim Semi fine Black Black Dark brown CNDI 06 3 Incision Rim Fine Reddish Reddish Sandwich structure with a black core CNDI 07 2 Impression Body Fine Reddish Greyish Light brown CNDI 08 2 None Body Semi fine Light grey Light grey Light brown CNDI 09 3 Carved roulette Rim with a lot of mica reflection Semi fine Dark red Dark brown Reddish CNDI 10 2 Incision/ tracing Rim Fine Greyish/grey Light grey Dark brown CNDI 11 2 Carved roulette Rim Semi fine Light grey Light grey Light brown CNDI 12 2 Impression Body Semi fine Light grey Light grey Light brown CNDI 13 2 Impression Body Fine Dark brown Dark grey/ Dark brown Page 6 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 The step size was 0.02° (2θ), whereas the time per step was 48 s. No internal standard was added to the powders. The qualitative identification of mineral phases was carried out using the XPowderX software [19]. According to Garside and Richardson [20], it is important to note that the interpretation of the diffraction pattern is hampered by phase mixing and the technique provides little useful information about the amorphous fraction. Thermogravimetry (TG) was used to study the thermal reactions of selected ceramics according to their mineralogy to complete the information obtained by PXRD. TG analysis was carried out with a Mettler Toledo TGA/ DSC1 apparatus. About 20 mg of sample was deposited on an Al crucible and analysed in a flowing air atmosphere (50 ml/min) at a heating rate of 20℃/min in the 25–950℃ temperature interval. For the petrographic study, one thin section per ceramic sample was prepared and observed under a Carl Zeiss Jenapol-U polarized optical microscope (POM). Images in the plane- and crossed-polarized light of the texture and mineralogy were captured with a Nikon D7000 digital camera. Colour measurements on the surfaces of ceramics were performed with a portable Konica Minolta CM-700d spectrophotometer to determine quantitatively their colour. Lightness (L*) and chromatic coordinates (a* and b*) were determined in the 400–700 nm wavelength range by selecting CIE illuminant D65 that simulates daylight with a colour temperature of 6504 K. Circular areas of the samples with a diameter of 3 mm were analysed (10° vision angle). The illumination was provided by a pulsed xenon lamp with UV cut filter, while a silicon photodiode array detected and measured both incidents and reflected light [21]. Water absorption and drying tests were carried out to assess the hydric behaviour of the ceramics. These tests provide valuable information on the porous system of the materials, predicting their greater or lesser susceptibility to degradation since saline solutions easily circulate through the pores and fissures of materials. The samples used for hydric tests were previously dried in an oven at 70 °C for 24 h to remove any possible moisture. Free water absorption (Ab), forced (under vacuum) water absorption (Af), drying index (Di), degree of pore interconnection (Ax) [22], open porosity (Po), saturation coefficient (S) and apparent (ρb) and real densities (ρsk) were calculated according to UNE-EN 13755 [23], NORMAL 29/88 [25] and RILEM [24] standards. Results anddiscussion Chemical composition SiO2 is the highest compound in all the studied samples. Seven samples (CNDI 05, 06, 07, 08, 10, 11 and 13) exceed 62 wt.%, and the other six are between 53 to 58 wt.% (Table2). This suggests the presence of quartz and other silicate phases in the studied ceramics. The Al2O3 content varies between 16 to 26 wt.% and seems to be related to the presence of phyllosilicates and feldspars s.l. [26]. The ratios SiO2/Al2O3 are greater than 2 and indicate the predominance of quartz over clay minerals [27, 28]. These and the following suggestions should be confirmed later, after mineralogical analysis of the samples (Sect. "Powder X-ray diffraction (PXRD) and thermogravimetry (TG)"). The ceramics are all CaO poor, being this compound comprised between 0.3 and 1.9 wt.% (Table2). Fe2O3 is quite high (around 11 wt.%) in three samples (CNDI 01, CNDI 02 and CNDI 09). Six samples (CNDI 03, CNDI 04, CNDI 06, CNDI 10, CNDI 12 and CNDI 13) have the Fe content comprised between 6 to 9 wt.%. The remaining four have Fe content of 3 to 4 wt.%. The high amount of iron content in CNDI 01, CNDI 02 and CNDI 09 justifies the marked red colour of these ceramics observed macroscopically and is maybe due to the presence of hematite [29, 30]. Concerning alkalis, the K2O content varies between 1.4 to 4 wt.% in all the samples, probably due to the presence of different amounts of K-feldspar and phyllosilicates [31, 32]. Na2O content is very low and negligible in all the samples. Fig. 4 Representative ceramics of the three macroscopic groups: A external surface; B internal surface 1) Group 1: sherd CNDI 05, 2) Group 2: sherd CNDI 08, 3) Group 3: sherd CNDI 01 (size of the square edge: 1 cm) Page 7 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 The percentage of flux oxides (K2O + Na2O + CaO) in all ceramics is low and consequently they are refractory because the high content of these elements will reduce their melting temperature. P2O5 values are in the range of 0.13—0.37 wt.%, except CNDI 05 sample, which shows content as high as 0.88 wt.%. A value higher than 0.5% generally suggests phosphorus contamination [33]. P2O5 could have come from a swamp area or cemetery and, therefore, could have been contaminated by infiltration of water during burial or by daily use [34, 35]. Moreover, CNDI 05 is the sample with the sample with the highest LOI content. According to the literature, values of LOI over 2% in CaO poor ceramics can be explained by the presence of water absorbed during the burial or by the dehydroxylation of clay minerals still present in ceramics due to firing at low temperatures [36, 37]. Table 3 shows the trace elements (in ppm) of the studied ceramics. The amount of Ba, Cr, Zr and V are high compared to the other measured elements (Table2). The high Ba content (468 to 1099ppm) can be explained by the presence of barite crystals or the contamination of the samples during the burial stage [34, 38]. The amount of Cr varies between 138 to 610ppm and most of the samples do not exceed 280ppm. The high Cr content in some samples (CNDI 01, CNDI 04, CNDI 10 and CNDI 12) can be explained by the presence of chromite. The amount of Zr varies between 152 and 444ppm and suggests the existence of zircon. V is in the range 90–278ppm and may indicate the formation of some vanadate compound. The variation of the major and trace elements of the studied samples does not appear to be correlated with the macroscopic classification. Table 2 chemical composition of major oxides (in wt.%) LOI stands for loss on ignition Samples Group SiO2Al2O3Fe2O3MnO MgO CaO Na2O K2OTiO2P2O5LOI CNDI 01 3 55.66 20.63 11.27 0.04 2.04 0.79 0.18 1.62 1.54 0.22 5.57 CNDI 02 3 53.21 23.35 11.44 0.08 1.58 0.82 0.56 3.91 2.27 0.21 1.89 CNDI 03 2 57.90 25.47 6.18 0.03 0.88 1.07 0.70 1.38 1.32 0.28 4.09 CNDI 04 2 56.77 25.91 7.29 0.03 1.95 1.83 0.79 1.34 0.79 0.37 2.15 CNDI 05 1 62.11 20.96 3.92 0.03 1.01 0.97 0.59 1.59 0.92 0.88 6.40 CNDI 06 3 63.88 18.39 6.30 0.05 1.25 0.69 0.13 3.36 1.84 0.31 3.11 CNDI 07 2 63.19 24.89 3.08 0.01 0.43 0.83 0.50 2.65 0.77 0.13 2.78 CNDI 08 2 66.25 20.70 3.76 0.03 0.65 0.64 0.15 2.12 2.20 0.19 2.57 CNDI 09 3 57.86 19.89 10.93 0.05 1.95 0.89 0.23 2.54 1.74 0.30 2.93 CNDI 10 2 62.76 19.64 9.10 0.03 1.44 0.78 0.22 1.43 1.30 0.30 2.57 CNDI 11 2 64.49 21.17 3.93 0.03 0.77 0.83 0.69 3.15 1.07 0.21 2.89 CNDI 12 2 58.07 25.41 6.20 0.02 0.68 0.89 0.12 2.82 1.65 0.33 3.02 CNDI 13 2 68.62 15.91 6.06 0.03 1.56 0.4 0.07 2.17 1.02 0.23 3.44 Table 3 Chemical composition of trace elements (in ppm) Samples Group Zr Sc VCr Co Ni Cu Zn Ga Rb Sr Y Nb Ba La Ce Nd Sm Pb Th CNDI 01 3 299 32 278 315 16 93 81 113 24 100 75 40 15 900 98 181 82 13 17 12 CNDI 02 3 256 64 227 160 21 80 50 150 28 165 123 50 21 788 85 154 81 15 19 11 CNDI 03 2 336 31 196 222 18 57 73 107 29 73 147 49 16 669 86 156 68 14 21 8 CNDI 04 2 152 29 118 610 24 73 49 109 23 71 151 28 11 1099 33 58 24 7 15 5 CNDI 05 1 295 18 133 161 12 39 26 84 25 113 96 30 11 554 103 189 68 10 19 32 CNDI 06 3 279 26 207 181 15 62 49 90 22 130 77 48 21 662 77 133 71 13 16 7 CNDI 07 2 348 10 90 170 4 53 15 67 34 111 169 19 17 581 67 116 43 9 45 19 CNDI 08 2 373 26 170 138 9 36 39 109 26 150 95 54 22 468 68 100 60 14 18 10 CNDI 09 3 319 36 230 275 16 79 53 115 26 140 83 65 20 737 107 197 98 21 13 15 CNDI 10 2 220 31 182 434 18 96 66 153 23 89 70 22 10 498 46 80 35 8 18 5 CNDI 11 2 444 12 155 247 17 45 22 81 27 138 142 29 20 581 70 135 52 10 28 20 CNDI 12 2 288 27 190 419 16 69 29 80 31 142 172 35 17 887 103 185 59 12 33 9 CNDI 13 2 249 20 156 145 10 41 35 79 17 104 41 28 13 497 40 76 34 8 14 8 Page 8 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 Powder X‑ray diffraction (PXRD) andthermogravimetry (TG) The X-ray diffraction patterns show that all the ceramic samples are rich in quartz (Qz) and contain feldspars s.l. (Fsp) (Fig. 5) confirming our suggestions based on the results of chemical analysis. Most of samples are also composed of muscovite (Ms), while kaolinite (Kln) and actinolite (Act) were only detected in CNDI 01 and CNDI 04, respectively. The differences in the mineralogy of samples lead to propose the existence of three new groups: – Mineralogical group 1: quartz + feldspar + kaolinite + muscovite (1 sample); – Mineralogical group 2: quartz + feldspar + muscovite (10 samples); – Mineralogical group 3: quartz + feldspar (2 samples). The differences detected in the three groups may imply changes in the use of raw materials, and/or more likely in the technology production (i.e., addition of temper and firing temperature). As the chemical analysis was unable to differentiate the thirteen samples into distinct groups, it is assumed that only one raw material was used. According to the mineral phases detected by PXRD, the ceramic from group 1 was probably fired below 600℃ due to the presence of kaolinite. As this phyllosilicate disappears between 400 and 650 °C [10, 35], its presence in the ceramic means that the firing temperature was not high enough to decompose it. The presence of muscovite in the ceramics (and the absence of kaolinite) from group 2 indicates a firing temperature over 600 ºC but below 900 °C because mica disappears around 900–1000°C [10, 35]. Its presence in the sherds means that their firing temperature was not high enough to decompose it. The third group of samples was fired over 900 °C due to the absence of phyllosilicates [39]. It is curious to note that the hematite is not detected even if the high Fe2O3 content determined by XRF. Probably, iron is present in ceramics in an amorphous or poorly crystalline phase. Based on the mineralogy identified by PXRD, three samples (CNDI 01, CNDI 07 and CNDI 13, i.e., one in each group) were selected to be investigated by thermogravimetry (TG). Figure 6 shows that the three samples present a slight mass loss up to 200 °C, which corresponds to the presence of hygroscopic water [40]. Sample CNDI 01 presents a second weight loss between 400–650℃ which is due to the loss of structural water contained in phyllosilicates [10, 40]. In fact, this is the only sample that contains kaolinite (Fig.5) and the loss is related to the dehydroxylation of this phyllosilicate, Fig. 5 PXRD patterns of the studied samples. Legend: Ms = muscovite; Kln = kaolinite; Act = actinolite; Qz = quartz; Fsp = feldspar s.l. Mineral abbreviations after Warr [42]. Black curve corresponds to the mineralogical Group1, blue curves to mineralogical Group 2 and red curves to mineralogical Group 3 Page 9 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 which turns into metakaolinite according to the following equation: CNDI 01 is the sample that loses the most weight by TG (6.7%) followed by CNDI 13 (3%) and CNDI 07 (2%), whose loss is really low and in agreement with the LOI values obtained by XRF (see Table2). The slightly higher value of weight loss in CNDI 13 compared to CNDI 07 is attributable to the residual dehydroxylation of the muscovite [41] present in the former, in agreement with PXRD data (Fig.6). The weight loss of the three samples in the sector with the greatest inflexion of the curves, i.e. between 450–720℃, is as follows: CNDI 01 loses 3.5% whereas the lowest weight loss is 0.8% for CNDI13 and 0.2% for CNDI 07. Polarized optical microscopy (POM) Figure7 shows the main features of the studied ceramics under optical microscopy. The petrographic analysis does not show the same grouping defined after macroscopic observations but agrees with the mineralogy determined by PXRD. All the ceramics are characterized by the presence of quartz, feldspar s.l. and phyllosilicates, which constitute the aplastic inclusions, in a matrix that varies from red to black. These aplastic inclusions appear poorly sorted in all the ceramics. Quartz is the main phase and appears as isolated crystals with undulose extinction and angular morphology Al 2 (OH) 4 (Si 2 O 5 ) → 2H 2 O + Al 2 O 3 .2SiO2 kaolinite water + metakaolinite or as part of gneiss fragments showing mosaic texture (Fig.7a). Feldspar s.l. is mainly constituted of K-feldspar with often signs of argillification (Fig. 7b) and sometimes cross-hatched twinning. Plagioclase with albitetype twinning is less frequent. Among phyllosilicates, muscovite is prevailing with first-to-second interference order colour, while biotite is sporadic (Fig.7c). These planar crystals are sometimes oriented due to the pressure exerted to the raw material during moulding (Fig.7a). Opaque minerals are scattered in the matrix of all samples. The pores are homogeneously distributed in the matrix and are mostly elongated. Some differences can be detected between samples based on the types or the aplastic inclusions, their abundance, sizes and the presence of accessory minerals. For example, CNDI 04 is the only sample where amphiboles were identified. Based on their colour, these inosilicates have low Fe content, being probably tremolite-actino- lite (Fig.7d). It is also the sample with the highest plagioclase content. Epidote s.s. has been observed in CNDI 11 (Fig. 7e), while small zircon crystals were detected in CNDI01 and CNDI 08 (Fig.7f). CNDI 06 highlights for the presence of a black core with red rims and a high amount of aplastic inclusions (Fig.7g). The opposite can be represented by CNDI 01, CNDI 02 and CNDI 12 due to their small grain size. CNDI 12 also shows red levels where small hematite crystals can be distinguished (Fig.7h). Some differences with the mineralogy identified by PXRD are due to the detection limit of the latter technique or because the crystals sizes are too low to be observed under POM. Physical analyses: porosity andcolour The studied samples have similar hydric behaviour with absorbed water between 18 and 24% (Ab, Table4). Only one sample, CNDI 05, is out of this range with a value of 14% (Fig.8 and Table4). This difference is maintained when samples undergo forced water absorption (Af, Table4). Regarding the degree of pore interconnection, CNDI 10 is the sample with the poorest pore interconnection (it has the highest Ax value, Table4) followed by CNDI 13, while CNDI 12, CNDI09 and CNDI 08 show the best pore interconnection (Ax ranges from 2 to 4) indicating easier water flow in the pore network of these three ceramics. The other samples range between 5 and 9. The drying of the ceramics (Di, Table4 and Fig.8) is very similar in all the samples (values ranging from 0.91 to 0.94), which indicates that they take almost the same time to dry. Samples that absorbed more water are those that generally attain higher open porosity values (Po, Table4). Porosity varies from 32 to 38%, being CNDI 05 the only Fig. 6 TG curves of three selected ceramic sherds. Black curve corresponds to CNDI 01 sample that contains kaolinite and muscovite; blue curve corresponds to CNDI 13 sample that contains muscovite; red curve corresponds to CNDI 07 sample that has no clay minerals and therefore is the one that lost the least weight Page 16 of 16 ZoilaLuzand Giuseppe Heritage Science (2024) 12:6 22. Cultrone G, Sebastian E, Elert K, Jose M, Cazalla O, Rodriguez NC. Influence of mineralogy and firing temperature on the porosity of bricks. J Eur Ceram Soc. 2004;24:547–64. 23. UNE-EN 13755. Métodos de ensayo para piedra natural. Determinación de la absorción de agua a presión atmosférica. AENOR. Madrid; 2008. 24. RILEM. Recommended test to measure the deterioration of stone and to assess the differences of treatment methods. Mater Struct. 1980;13:175–253. 25. NORMAL 29/88. Misura dell’indice di asciugamento (drying index). Rome, ICR-CNR; 1988. 26. Kramar S, Lux J, Mladenović A, Pristacz H, Mirtič B, Sagadin M, Smuč´NR. Mineralogical and geochemical characteristics of Roman pottery from an archaeological site near Mošnje (Slovenia). Appl Clay Sci. 2012;57:39–48. 27. Ndjigui PD, Mbey JA, Fadil-Djenabou S, Onana VL, Bayiga EC, Enock Embom C, Ekosso IG. Characteristics of kaolinitic raw materials from the lokoundje river (Kribi, cameroon) for ceramic applications. Appl Sci. 2021;11(13):6118. 28. Kılıç NÇ, Kılıç S, Akgül HÇ. An archaeometric study of provenance and firing technology of halaf pottery from tilkitepe (Eastern Turkey). Mediterr Archaeol Archaeom. 2017;17(2):35–48. 29. Palanivel R, Kumar UR. Thermal and spectroscopic analysis of ancient potteries. Rom J Phys. 2011;56(1–2):195–208. 30. De Bonis A, Cultrone G, Grifa C, Langella A, Leone AP. Different shades of red : The complexity of mineralogical and physico—chemical factors influencing the colour of ceramics. Ceram Int. 2017;43:8065–74. 31. Daghmehchi M, Rathossi C, Omrani H, Emami M, Rahbar M. Mineralogical and thermal analyses of the Hellenistic ceramics from Laodicea Temple. Iran Appl Clay Sci. 2018;65:146–54. 32. İssi A, Kara A, Alp AO. An investigation of Hellenistic period pottery production technology from Harabebezikan/Turkey. Ceram Int. 2011;37(7):2575–82. 33. Fabbri B, Gualtieri S. Reasons of phosphorus pollution inarchaeological pottery and its consequences: a reassessment. Dev Archaeol Res M Adalslteinn T Olander (eds), Nov Sci Publ New York. 2013;41–66. 34. Maggetti M. Chemical analyses of ancient ceramics : what for? Chimia. 2001;55(No 11):923–30. 35. Bonzon J. Archaeometrical study (petrography, mineralogy and chemistry) of Neolithic ceramics from Arbon Bleiche 3 (Canton of Thurgan, Switzerland). Suisse.: Université de Fribourg; 2005. 36. Fabbri B, Gualtieri S, Shoval S. The presence of calcite in archaeological ceramics. J Eur Ceram Soc. 2014;34:1899–911. 37. Camarda L, Cerchi E, Fabbri B, Gualtieri S, Verardi G. Classification and typology of the pottery from Gotihawa (nepalese Tarai), with particular reference to NBPW. In: Proceedings of the “South Asian Archaeology 2001”, Paris,. 2001. p. 35–9. 38. Ruffieux M. la production céramique entre le 9 et le 5 ème siècle avant JC dans le Broye. Cah d’ Archeol fribourgeoise. 2005; (N7 Etudes). 39. Cultrone G, Javier F, Rosua C. Applied clay science growth of metastable phases during brick firing : Mineralogical and microtextural changes induced by the composition of the raw material and the presence of additives. Appl Clay Sci. 2020;185: 105419. 40. Meyvel S, Satha P, Velraj G. Thermal characterization of archaeological potsherds recently excavated in Nedunkur, Tamilnadu. India Cerâmica. 2012;58:338–41. 41. Cultrone G. The use of Mount Etna volcanic ash in the production of bricks with good physical-mechanical performance: converting a problematic waste product into a resource for the construction industry. Ceram Int. 2022;48(4):5724–36. 42. Warr LN. IMA–CNMNC approved mineral symbols. Mineral Mag. 2021;85(3):291–320. 43. Oudbashi O, Naseri R, Cultrone G, Egartner I, Arizzi A. The pottery production from the Deh Dumen Bronze age graveyard (South-Western Iran): a chemical, mineralogical and physical study. Herit Sci. 2021;9(1):1–19. 44. Singh P, Sharma S. Journal of archaeological science : reports thermal and spectroscopic characterization of archeological pottery from Ambari. Assam JASREP. 2016;5:557–63. 45. Colomban P. Glasses, ceramics and enamelled objects. In: Garside; P, Richardson E, editors. Conservation Science: Heritage Materials. Royal Society of Chemistry; 2021. p. 478. 46. Daghmehchi M, Coletti C, Hyeok Moon D, Esmaeili Jelodar ME, Omrani H, Reka AA, Nematollahzadeh A, Emami M. Mineralogical and microstructural characterization of ceramics from the fifth and fourth millennium BC in the central plateau of Iran. Open Ceram. 2023;15: 100427. 47. Le Maitre RW. The chemical variability of some common igneous rocks. J Petrol. 1976;17:589–637. 48. Nockolds SR, Allen R. The geochemistry of some igneous rock series. Geochim Cosmochim Acta. 1953;4:105–42. 49. Mercader J, Garcia-Heras M, Gonzalez-Alvarez I. Ceramic tradition in the African forest: characterisation analysis of ancient and modern pottery from Ituri, DR: Congo. J Archaeol Sci. 2000;27:163–82. 50. Tsoupra A, Clist B, da Conceição LM, Moita P, Barrulas P, da Piedade JM, da Silva D, Bostoen K, Mirao J. A multi-analytical characterization of fourteenth to eighteenth century pottery from the Kongo kingdom, Central Africa. Sci Rep. 2022;12(1):1–18. 51. Livingstone SA. Chaîne opératoire de la poterie: références ethnographiques, analyses et reconstitution, vol. 1. Thèse Université Libre de Bruxelles: Musée Royale de l’Afrique Centrale. Université Libre de Bruxelles; 2001. 52. Gosselain OP. Poteries du Cameroun méridional. Styles techniques et rapports á l’identité. Editions C N R S Paris; 2002. 254 p. 53. Stahl AB, das Dores Cruz M, Neff H, Glascock MD, Speakman RJ, Giles B, Smith L. Ceramic production, consumption and exchange in the Banda area, Ghana: Insights from compositional analyses. J Anthropol Archaeol. 2008;27(3):363–81. Publisher’s Note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.