Crystallization, Luminescence and Cytocompatibility of Hexagonal Calcium Doped Terbium Phosphate Hydrate Nanoparticles
Abstract
Spanish Agencia Estatal de Investigación of the Ministerio de Ciencia, Innovación y Universidades (MICIU)
Full text
nanomaterials Article Crystallization, Luminescence and Cytocompatibility of Hexagonal Calcium Doped Terbium Phosphate Hydrate Nanoparticles Jaime Gómez-Morales 1,* , Raquel Fernández-Penas 1, Ismael Romero-Castillo 1, Cristóbal Verdugo-Escamilla 1, Duane Choquesillo-Lazarte 1, Annarita D’Urso 2, Maria Prat 2,3,4,5,* and Jorge Fernando Fernández-Sánchez 6 Citation: Gómez-Morales, J.; Fernández-Penas, R.; Romero-Castillo, I.; Verdugo-Escamilla, C.; Choquesillo-Lazarte, D.; D’Urso, A.; Prat, M.; Fernández-Sánchez, J.F. Crystallization, Luminescence and Cytocompatibility of Hexagonal Calcium Doped Terbium Phosphate Hydrate Nanoparticles. Nanomaterials 2021,11, 322. https://doi.org/ 10.3390/nano11020322 Academic Editor: Marie-Helene Delville Received: 24 December 2020 Accepted: 21 January 2021 Published: 27 January 2021 Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations. Copyright: © 2021 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (https:// creativecommons.org/licenses/by/ 4.0/). 1 Laboratorio de Estudios Cristalográficos, IACT, CSIC-UGR, Avda. Las Palmeras, n º 4, 18100 Granada, Spain; [email protected] (R.F.-P.); [email protected] (I.R.-C.); cristobal.ver[email protected] (C.V.-E.); [email protected] (D.C.-L.) 2 Dipartimento di Scienze della Salute, Universitàdel Piemonte Orientale, Via Solaroli, 17, 28100 Novara, Italy; [email protected] 3Centro di Biotecnologie per la Ricerca Medica Applicata (BRMA), Via Solaroli 17, 28100 Novara, Italy 4Consorzio Interuniversitario per Biotecnologie (CIB), LocalitàPadriciano 99, 34149 Area di Ricerca, Italy 5 Consorzio Interuniversitario Nazionale per la Scienza e Tecnologia dei Materiali (INSTM), 28100 Novara, Italy 6Department of Analytical Chemistry, Faculty of Sciences, University of Granada, Avda. Fuentenueva s/n, 18071 Granada, Spain; [email protected] * Correspondence: [email protected] (J.G.-M.); [email protected] (M.P.); Tel.: +34-958-230000 (J.G.-M.); +39-0321-660662(M.P.) Abstract: Luminescent lanthanide-containing biocompatible nanosystems represent promising candidates as nanoplatforms for bioimaging applications. Herein, citrate-functionalized calcium-doped terbium phosphate hydrate nanophosphors of the rhabdophane type were prepared at different synthesis times and different Ca 2+ /Tb 3+ ratios by a bioinspired crystallization method consisting of thermal decomplexing of Ca 2+ /Tb 3+ /citrate/phosphate/carbonate solutions. Nanoparticles were characterized by XRD, TEM, SEM, HR-TEM, FTIR, Raman, Thermogravimetry, inductively coupled plasma spectroscopy, thermoanalysis, dynamic light scattering, electrophoretic mobility, and fluorescence spectroscopy. They displayed ill-defined isometric morphologies with sizes ≤ 50 nm, hydration number n ~ 0.9, tailored Ca 2+ content (0.42–8.11 wt%), and long luminescent lifetimes (800–2600 µ s). Their relative luminescence intensities in solid state are neither affected by Ca 2+ , citrate content, nor by maturation time for Ca 2+ doping concentration in solution below 0.07 M Ca 2+ . Only at this doping concentration does the maturation time strongly affect this property, decreasing it. In aqueous suspensions, neither pH nor ionic strength nor temperature affect their luminescence properties. All the nanoparticles displayed high cytocompatibility on two human carcinoma cell lines and cell viability correlated positively with the amount of doping Ca 2+ . Thus, these nanocrystals represent promising new luminescent nanoprobes for potential biomedical applications and, if coupled with targeting and therapeutic moieties, they could be effective tools for theranostics. Keywords: terbiumphosphates; calciumdoped; citrate; nanoparticles; luminescence; cytocompatibility 1. Introduction Luminescent nanoparticles are excellent optical probes for uses in biological imaging since they provide the essential fluorescent contrast to analyze and study cells and tissues [ 1 ]. Different luminescent labeling agents, mainly organic dyes, and nanomaterials including semiconductor quantum dots, nanodiamonds, gold nanoparticles [ 2 – 4 ], several nanostructures labeled with organic dyes [ 5 ], and more recently calcium phosphate apatite nanoparticles (nAp) both labeled with organic dyes [ 6 ] or doped with luminescent lanthanides (Ln 3+ ) ions [ 7 , 8 ], have been proposed for these applications. The main limitation of organic dyes is photobleaching [ 5 ], while the use of quantum dots is controversial due Nanomaterials 2021,11, 322. https://doi.org/10.3390/nano11020322 https://www.mdpi.com/journal/nanomaterials
Nanomaterials 2021,11, 322 2 of 19 to their cytotoxicity [ 9 ]. In the last years lanthanide orthophosphates (LnPO 4 , Ln 3+ = Eu 3+ , Tb 3+ , Ce 3+ , Y 3+ . . . ) started to attract much attention because they combine the very low solubility and high thermal conductivity of the metal phosphates as host matrices with the favorable features of the luminescent lanthanide ions, such as sharp emission bands, Stokes shift of hundreds of nanometers, and luminescence lifetimes of the order of milliseconds. For all the above reasons they find applications as phosphors, catalysts, sensors and heatresistant materials [ 10 ]. In addition, they exhibit low cytotoxicity, high photostability, and resistance to photobleaching, thus being good optical nanoprobes for bioimaging [ 11 – 13 ]. LnPO 4· nH 2 O (n= 0–2) presents five polymorphic modifications, among which the low temperature hydrated phase with hexagonal structure is known as raphdophane [ 14 , 15 ]. In respect to Ln 3+ -doped nAp, the LnPO 4· nH 2 O system presents the main advantage that at low temperatures (<100 ◦ C) raphdophane is usually the only precipitated phase from aqueous solutions [ 15 ]. In calcium phosphate solutions, in contrast, several polymorphs can eventually appear including amorphous calcium phosphate (ACP), dicalcium phosphate dihydrate (DCPD, brushite), octacalcium phosphate (OCP), and Ap [ 16 – 18 ]. The synthetic methods to prepare LnPO 4 nanocrystals include hydrothermal crystallization [ 19 – 21 ], microwave heating [ 22 ], ultrasounds [ 23 ], oil bath [ 24 ], sol-gel combined with electrospinning [ 25 ], slow crystallization using surfactants [ 26 ], or the layer-by layer adsorption followed by the reaction and crystallization at room temperature [27]. Among lanthanides, Eu 3+ and Tb 3+ started to be used in various host structures using different excitation wavelength in the UV region, with main emission bands in the Visible spectral region. Concerning LnPO 4 , the TbPO 4· nH 2 O raphdophane nanorods were excited in the UV region at either 270, 312, 350 or 370 nm, and in the visible region at 482 nm , resulting in similar emission spectra, and yielding a characteristic green emission, due to 5 D 4 – 7 F 5 transition at 546 nm emission of Tb 3+ [ 28 ]. Doping with Eu 3+ allows the preparation of Eu 3+ : TbPO 4 of hexagonal form with improved energy transfer efficiency between Tb 3+ and Eu 3+ and non-cytotoxicity on HeLa cells [ 13 ]. Recently, our group used citrate (cit) to prepare new luminescent cit-coated Ca 2+ :EuPO 4· nH 2 O (with n~1) by the method of thermal decomplexing of M (2+/3+) /Ca 2+ /cit/phosphate/carbonate solutions (M (2+/3+) , metallic ions) [ 29 ]. The method was initially developed to precipitate monodisperse biomimetic apatites [ 30 ] and carbonated apatite nanocrystals, both undoped and doped with transition metals [ 31 , 32 ], and Eu 3+ [ 8 ]. In this method citrate ions played an active role in the nucleation and growth steps, and remained adsorbed on the nanoparticles surface [ 33 ], a feature presented in bone apatite nanocrystals [ 34 ]. The new luminescent cit-Ca 2+ :EuPO 4· H 2 O nanomaterials proved to be fully cytocompatible against GTL-16 human carcinoma cells and showed an improved cytocompatibility as the Ca 2+ content increased when contacted with the more sensitive m17.ASC murine mesenchymal stem cells, thus proving to be suitable for bioimaging and cell labeling. The aim of the present work is to employ the same bioinspired route to prepare cit- Ca 2+ :TbPO 4· nH 2 O nanocrystals with tuned luminescence and high cytocompatibility, in the assumption that the presence of Ca 2+ in the structure and citrate adsorbed on these luminescent solids must be beneficial from the point of view of the cytocompatibility required in bioimaging. 2. Materials and Methods 2.1. Materials and Precipitation Method For the experiments the following reagents were purchased from Sigma-Aldrich ( St Louis , MO, USA): Terbium (III) chloride anhydrous (TbCl 3 , 99.9% pure, trace metals), sodium citrate tribasic dihydrate (Na 3 (cit) · 2H 2 O, where cit = citrate = C 6 H 5 O 7 , ACS reagent, ≥ 99.0% pure), calcium chloride dihydrate (CaCl 2· 2H 2 O, Bioxtra, ≥ 99.0% pure), and sodium phosphate dibasic (Na 2 HPO 4 , ACS reagent, ≥ 99.0% pure). Sodium carbonate monohydrate (Na 2 CO 3· H 2 O, ACS reagent, 99.5% pure) and hydrochloric acid (HCl, ACS reagent, 37 wt % in H 2 O) were provided by Merck (Darmstadt, Germany) and Panreac
Nanomaterials 2021,11, 322 3 of 19 (Barcelona, Spain), respectively. Solutions were prepared with ultrapure deionized water (0.22 µS, 25 ◦C, Milli-Q, Millipore, Burlington, MA, USA). The synthesis of nanocrystals was carried out by the already established method of thermal decomplexing of M (2+/3+) /Ca 2+ /cit/phosphate/carbonate solutions [ 29 ], using Tb 3+ as lanthanide ion (y= 0.09, 0.07, 0.05 and 0.03 M) and increasing concentrations of doping Ca 2+ in the solution (x= 0.01 M, 0.03, 0.05, and 0.07 M) to set x+y= 0.1 M. The experiments lasted 4 h, 24 h, and 96 h. Some of them were matured for 7 days. The precipitates were subjected to washing by centrifugation with ultrapure water (6 cycles, 9000 rpm, 9 min each) and freeze-dried overnight at −50 ◦C under vacuum (3 mbar). 2.2. Physico-Chemical Characterization of Solid Nanoparticles As-prepared powders were analyzed by different techniques, as it is described below: X-ray powder diffraction (XRD) patterns were recorded using a diffractometer PANA- lytical MPD (PANAlytical, Almelo, The Netherlands) with a Bragg-Brentano parafocusing geometry and Cu K α radiation. Data processing of most matured samples was carried out with software TOPAS 6.0 (Coelho Software, Brisbane, Australia) [ 35 ]. The contribution of the isotropic peak broadening due to domain size was modeled using the “CS_L” TOPAS macro based on the Scherrer approximation, and considering the instrumental contribution from a measurement of LaB6standard (NIST SRM 660c). TEM observations were performed with a TEM Libra 120 Plus (EELS) instrument at 80 kV (Carl Zeiss, Jena, Germany). Prior to observation samples were dispersed in absolute ethanol ( ≥ 99.8% v/v) and deposited on copper microgrids coated with FORMVAR carbon film. HRTEM analysis were done with a TITAN G2 60-300 FEI Instrument (FEI, Hillsboro, OR, USA) operating at 300 kV, equipped with EDX Super X detector to perform microanalysis, and STEM type HAADF. Fourier transform infrared spectra (FTIR) were recorded in transmittance mode within the wavelength range from 4000 cm −1 to 400 cm −1 using a Perkin-Elmer Spectrum One FTIR spectrometer (Perkin Elmer, Shelton, WA, USA). Pellets with ~1 wt% sample in anhydrous KBr were prepared and pressed with a hydraulic pump at 10 tons. Pure KBr pellets were used to record the background. Raman spectra were recorded with a LabRAM HR spectrometer (Jobin–Yvon, Horiba, Tokyo, Japan). The excitation line was provided by a diode laser emitting at a wavelength of 532 nm while a Peltier cooled charge–couple device (CCD) (1064 ×256 pixels) was used as a detector. Crystal size distribution (CSD) and electrophoretic mobility ( ζ -potential) were analyzed with a Zetasizer Nano ZS analyzer (Malvern Instruments Ltd., Malvern, UK) in aqueous suspensions (~0.5 mg/mL, 25 ◦ C) contained in disposable polystyrene cuvettes. For ζ -potential versus pH measurements the MPT-2 autotitrator ( Malvern Instruments Ltd. , Malvern, UK) was employed to adjust the pH of the suspensions. Diluted HCl and NaOH solutions (0.25 and 0.1 M, respectively) were used as titration agents without any additional electrolyte. Elemental analysis of Tb was carried out by inductively coupled plasma mass spectroscopy (ICP MS) using a Perkin Elmer NexION 300D ICP Mass spectrometer (Perkin Elmer). Ca and P were analyzed with Perkin Elmer ICP-OES OPTIMA 8300 spectrometer (Perkin Elmer); C and H were determined by thermoanalysis using Thermo Scientific ™ FLASH 2000 CHNS/O Analyzer of Thermo Fisher Scientific (Waltham, MA, USA). TGA analyses were performed with a thermogravimetric analyzer TGA-50H model (Shimadzu, Tokyo, Japan). Samples were weighted in a platinum crucible and heated from room temperature (~28 ◦C) to 950 ◦C under 50 mL/min air flow with a heating rate of 20 ◦C/min. 2.3. Luminescence Spectroscopy Excitation and emission spectra of both powder and aqueous suspension mg/mL samples, the latter being at ~0.5 mg/mL, were recorded using a Cary Eclipse Varian Fluorescence Spectrophotometer (Varian Australia, Mulgrave, Australia) using λexc = 375 nm , λem = 545 nm, 0.120 µ s delay time (td) and 5 ms gate time (t g ); photomultiplier voltage
Nanomaterials 2021,11, 322 4 of 19 of 470 V and slit width exc/em 5/5 nm for powder samples and photomultiplier voltage of 800 V and slit width exc/em 10/10 nm for aqueous suspension particles. The excitation and emission spectra were recorded within the range 250–500 nm and 500–750 nm, respectively. Lifetime ( τ ) measurements were also recorded by a Cary Eclipse Varian Fluorescence Spectrophotometer (Varian Australia, Mulgrave, Australia) using λexc/em = 375/475 nm, 100 µ s delay time (t d ), 0.010 ms gate time (t g ), photomultiplier voltage of 600 V, slit width exc/em 10/10 nm and 100 cycles. For solid sample analysis, a Cary Eclipse Solid Sample Holder (https://www.agilent.com/ en/product/molecular-spectroscopy/fluorescence-spectroscopy/fluorescence-accessories/caryeclipse-solid-sample-holder) was used to allow the measuring at the optimum angle and to minimize the effect of the thickness. Concerning the dispersity of the measurements, they are not shown in the figures due to their lower value. In all the case the RSD (relative standard deviation) were lower than 2% (n= 3). 2.4. Cytocompatibility Tests Nanocrystal cytocompatibility was tested on two cell lines: GTL-16 (a human gastric carcinoma cell line) and A549 (a human lung adenocarcinoma cell line). Then, 24 h after seeding cells (12,000 GTL-16 and 5000 A549 cells/well in 96-well plates), different concentrations of the differentially doped (x= 0.01, 0.03, 0.05, 0.07 M Ca 2+ ) nanoparticles, ranging from 0.1 to 100 mg/mL, were added in 100 mL of fresh medium. Hydrogen peroxide ( 1 mM ) was used as control of toxicity. After 72 h incubation, cell viability was evaluated by the 3-(4,5-Dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide) ( MTT, Sigma ) colorimetric assay. Briefly, 20 mL of MTT solution (5 mg/mL in a PBS solution) were added to each well and the plate was incubated at 37 ◦ C for 3 h. After the removal of the solution, 125 mL of isopropanol, 0.2 M HCl was added to dissolve formazan crystals. One hundred mL were then removed carefully, and the optical density was measured in a multiwell reader ( 2030 Multilabel Reader Victor TM X4, Perkin Elmer) at 570 nm. Viability of parallel cultures of untreated cells was taken as 100% viability, and values obtained from cells undergoing the different treatments were referred to this value. Experiments were performed 3 times using 3 replicates for each sample. Data were statistically analyzed and are expressed as mean ± standard deviation. Statistical analyses were performed using a oneway ANOVA with Bonferroni’s post-hoc test for grouped analyses using GraphPad Prism version 4.03 for Windows, GraphPad Software (GraphPad Prism, San Diego, CA, USA ). Differences at p< 0.05 were considered to be statistically significant. 3. Results 3.1. Structural, Physicochemical, Morphological Characteristics, and Colloidal Stability of Solid Nanoparticles The XRD patterns of the solids precipitated for increasing concentration of Ca 2+ (x, from 0.01 M to 0.07 M) and increasing maturation times (from 4 to 96 h) are reported in Figure 1. In particular, the patterns showing the distinguishing reflections of the hexagonal (raphdophane) phase identified as TbPO 4· nH 2 O, space group P3 1 21 (PDF 20 1244) are displayed in panels a–d. At x= 0.01 M Ca 2+ this is the only crystalline phase identified. The main reflections of this phase are located at 2 θ 14.85 ◦ (100), 20.43 ◦ (101), 25.91 ◦ (110), 30.02 ◦ (200), 32.10 ◦ (102), 38.72 ◦ (112), 42.70 ◦ (003), 48.10 ◦ (301), 49.63 ◦ (212), 53.2 ◦ (203), and 54.5 ◦ (302). Other minor reflections (non-indexed) appear beyond 2 θ 55 ◦ . These latter peaks are not shown in the PDF 20-1244 card, but are similar to those appearing in the PDF 20-1044 card corresponding to the raphdophane structure in the EuPO4·H2O. In addition, small differences in 2 θ positions are found between the two patterns because some peak assignments in PDF file 20 1244 are affected with errors ≥ 0.2 ◦ . When x ≥ 0.03 M Ca 2+ (Figure 1b–d), however, an additional phase started to crystallize. The reflections of this phase at ~27 ◦ and 32.8 ◦ are assigned to CaCO 3 vaterite (PDF 33-0268), possibly doped with terbium. The presence of vaterite is more evident at x= 0.05 and 0.07 M Ca 2+ . Thus, this
Nanomaterials 2021,11, 322 5 of 19 compound becomes stable in calcium-rich medium due to the presence of residual CO 32− in the crystallizing solutions. Nevertheless, its presence does not represent a problem concerning biomedical uses since this polymorph of CaCO 3 is biocompatible [ 36 ]. At 0.07 M Ca 2+ we found a slightly different phase evolution with time. At 4 h, the bulging of the baseline is characteristic of an amorphous phase, probably of terbium phosphate, whereas at 24 h the reflections of the raphdophane phase started to emerge from the bulging baseline. In none of the experiments have we detected the presence of any calcium phosphate phase. Nanomaterials 2021, 10, x FOR PEER REVIEW 5 of 19 card corresponding to the raphdophane structure in the EuPO 4 ·H 2 O. In addition, small differences in 2θ positions are found between the two patterns because some peak assignments in PDF file 20 1244 are affected with errors ≥ 0.2°. When x ≥ 0.03 M Ca 2+ (Figure 1b– d), however, an additional phase started to crystallize. The reflections of this phase at ~27° and 32.8° are assigned to CaCO 3 vaterite (PDF 33-0268), possibly doped with terbium. The presence of vaterite is more evident at x = 0.05 and 0.07 M Ca 2+ . Thus, this compound becomes stable in calcium-rich medium due to the presence of residual CO 32− in the crystallizing solutions. Nevertheless, its presence does not represent a problem concerning biomedical uses since this polymorph of CaCO 3 is biocompatible [36]. At 0.07 M Ca 2+ we found a slightly different phase evolution with time. At 4 h, the bulging of the baseline is characteristic of an amorphous phase, probably of terbium phosphate, whereas at 24 h the reflections of the raphdophane phase started to emerge from the bulging baseline. In none of the experiments have we detected the presence of any calcium phosphate phase. Figure 1. Evolution of XRD patterns with maturation time (4 h, green; 24 h, red; 96 h, blue) of samples precipitated from Ca 2+ /Tb 3+ /cit/phosphate/carbonate solutions in presence of increasing concentrations of Ca 2+ : (a) x = 0.01 M Ca 2+ ; (b) x = 0.03 M Ca 2+ ; (c) x = 0.05 M Ca 2+ , and (d) x = 0.07 M Ca 2+ . * hexagonal phase TbPO 4 ·nH 2 O PDF 20-1244. The microstructural study of 96 h samples was performed by analysis of the full XRD pattern, excluding the reflections of vaterite (Figure 2). Results show isometric crystalline domains whose average Scherrer diameters were 37.6 ± 0.2 nm for the less Ca 2+ -doped sample (Figure 2a), 28.6 ± 0.2 nm for x = 0.03 M Ca 2+ (Figure 2b), 24.9 ± 0.2 for x = 0.05 (Figure 2c), and 30.2 ± 0.1 for x = 0.07 M Ca 2+ (Figure 2d), respectively. Figure 1. Evolution of XRD patterns with maturation time (4 h, green; 24 h, red; 96 h, blue) of samples precipitated from Ca 2+ /Tb 3+ /cit/phosphate/carbonate solutions in presence of increasing concentrations of Ca 2+ : ( a )x= 0.01 M Ca 2+ ; ( b ) x= 0.03 M Ca2+; (c)x= 0.05 M Ca2+, and (d)x= 0.07 M Ca2+. * hexagonal phase TbPO4·nH2O PDF 20-1244. The microstructural study of 96 h samples was performed by analysis of the full XRD pattern, excluding the reflections of vaterite (Figure 2). Results show isometric crystalline domains whose average Scherrer diameters were 37.6 ± 0.2 nm for the less Ca 2+ -doped sample (Figure 2a), 28.6 ± 0.2 nm for x= 0.03 M Ca 2+ (Figure 2b), 24.9 ± 0.2 for x= 0.05 (Figure 2c), and 30.2 ±0.1 for x= 0.07 M Ca2+ (Figure 2d), respectively. TEM observations of these precipitates show nanocrystals with ill-defined shapes and aspect ratios close to 1 (Figure 3a–c). In contrast to what has been reported for cit- Ca 2+ :EuPO 4· H 2 O nanoparticles, no appreciable dependence of their morphology with Ca 2+ doping was found [29].
Nanomaterials 2021,11, 322 6 of 19 Nanomaterials 2021, 10, x FOR PEER REVIEW 6 of 19 Figure 2. Crystalline domain sizes of Ca 2+ :TbPO 4 ·nH 2 O nanoparticles prepared with, (a) x = 0.01 M; (b) x = 0.03 M; (c) x = 0.05 M and (d) x = 0.07 M Ca 2+ for 96 h, calculated by analysis of the full XRD pattern using TOPAS 6.0. The two XRD vaterite reflections are excluded. R wp , weighted profile R-factor as described in Young [37]. TEM observations of these precipitates show nanocrystals with ill-defined shapes and aspect ratios close to 1 (Figure 3a–c). In contrast to what has been reported for cit- Ca 2+ :EuPO 4 ·H 2 O nanoparticles, no appreciable dependence of their morphology with Ca 2+ doping was found [29]. Figure 2. Crystalline domain sizes of Ca 2+ :TbPO 4· nH 2 O nanoparticles prepared with, ( a )x= 0.01 M; ( b )x= 0.03 M; ( c ) x= 0.05 M and ( d )x= 0.07 M Ca 2+ for 96 h, calculated by analysis of the full XRD pattern using TOPAS 6.0. The two XRD vaterite reflections are excluded. Rwp, weighted profile R-factor as described in Young [37]. The sizes deduced on the basis of either TEM (29 ± 5, 28 ± 3, 33 ± 6, Figure 3a–c) or SEM (x= 0.07 M Ca 2+ , L = 55 ± 20 nm, not shown) images are equivalent to those measured from XRD data. The indexed SAED patterns (insets) show the crystallographic planes of the hexagonal phase, i.e., (100), (110) in Figure 3a, or (100), (102), (200) in Figure 3c. The sample obtained for x= 0.01 Ca 2+ was studied in more details, as shown in Figure 3d–i. Figure 3d displays the image in high angle annular dark field (HAADF) in Scanning Transmission Electron Microscopy (STEM). The elemental mappings composition of the nanoparticles (Figure 3e,f,h,i) show a homogeneous distribution of Tb, Ca, P, and O. HRTEM images of this sample (Figure 3g) reveal lattice fringes, basically monodomains, whose d-spacing of 2.78 Å corresponds to plane (102), also shown in the fast Fourier transform FFT images of this sample (Figure 3d, inset). FTIR and Raman spectroscopy were employed to reveal the spectroscopic features of the Ca 2+ -doped samples (see Figure 4for the stacking of spectra of precipitates prepared at different Ca 2+ doping concentrations, and Supplementary Figures S1 and S2 for the stackings as a function of maturation time).
Nanomaterials 2021,11, 322 7 of 19 Nanomaterials 2021, 10, x FOR PEER REVIEW 7 of 19 Figure 3. (a–c) TEM micrographs of cit-Ca 2+ :TbPO 4 ·H 2 O nanorods prepared with different Ca 2+ doping concentrations at 96 h: (a) x = 0.01 M; (b) x = 0.03 M; (c) x = 0.05 M. Insets display SAED patterns of the nanoparticles. (d) HAADF-STEM micrograph of sample x = 0.01 M Ca 2+ . (e,f,h,i) EDX element mapping analysis of Tb, Ca, P, and O in nanoparticles of image (d). (g) HR-TEM image showing lattice fringes and d-spacing of 2.78 Å corresponding to plane (102) of nanocrystals of sample x = 0.01 M Ca 2+ . Inset in g) shows the corresponding Fourier transform (FFT) image displaying the (102) plane. The sizes deduced on the basis of either TEM (29 ± 5, 28 ± 3, 33 ± 6, Figure 3a–c) or SEM (x = 0.07 M Ca 2+ , L = 55 ± 20 nm, not shown) images are equivalent to those measured from XRD data. The indexed SAED patterns (insets) show the crystallographic planes of the hexagonal phase, i.e., (100), (110) in Figure 3a, or (100), (102), (200) in Figure 3c. The sample obtained for x = 0.01 Ca 2+ was studied in more details, as shown in Figure 3d–i. Figure 3d displays the image in high angle annular dark field (HAADF) in Scanning Transmission Electron Microscopy (STEM). The elemental mappings composition of the nanoparticles (Figure 3e,f,h,i) show a homogeneous distribution of Tb, Ca, P, and O. HRTEM images of this sample (Figure 3g) reveal lattice fringes, basically monodomains, whose d-spacing of 2.78 Å corresponds to plane (102), also shown in the fast Fourier transform FFT images of this sample (Figure 3d, inset). FTIR and Raman spectroscopy were employed to reveal the spectroscopic features of the Ca 2+ -doped samples (see Figure 4 for the stacking of spectra of precipitates prepared at different Ca 2+ doping concentrations, and Supplementary Figures S1 and S2 for the stackings as a function of maturation time). Figure 3. ( a – c ) TEM micrographs of cit-Ca 2+ :TbPO 4· H 2 O nanorods prepared with different Ca 2+ doping concentrations at 96 h: ( a )x= 0.01 M; ( b )x= 0.03 M; ( c )x= 0.05 M. Insets display SAED patterns of the nanoparticles. ( d ) HAADF-STEM micrograph of sample x= 0.01 M Ca 2+ . ( e , f , h , i ) EDX element mapping analysis of Tb, Ca, P, and O in nanoparticles of image ( d ). ( g ) HR-TEM image showing lattice fringes and d-spacing of 2.78 Å corresponding to plane (102) of nanocrystals of sample x= 0.01 M Ca2+. Inset in (g) shows the corresponding Fourier transform (FFT) image displaying the (102) plane. Nanomaterials 2021, 10, x FOR PEER REVIEW 8 of 19 Figure 4. (a) FTIR and (b) Raman spectra of samples precipitated at 96 h using Ca 2+ -doping concentrations x = 0.01 M (purple), x = 0.03 M (green), x = 0.05 M (red), x = 0.07 M (light blue). FTIR spectra of Ca 2+ -doped samples (Figure 4a) show basically the same spectroscopic features upon calcium doping, especially for x = 0.01, 0.03, and 0.05 M Ca 2+ . These are a broadband between 3600–3700 cm −1 and 2600 cm −1 corresponding to the O–H stretching of associated water, a main broad band at 1000–1100 cm −1 , which corresponds to the antisymmetric stretching mode of PO 43− groups (ν 3 PO 4 ) and two intense bands at ~620 and 535 cm −1 ascribed to the bending mode of the same PO 43− groups (ν 4 PO4). The broader signals around 1590–1620 cm −1 and 1405–1430 cm −1 are assignable to the antisymmetric and symmetric stretching frequencies of carboxylate (−COO − ) groups of the adsorbed citrate [29]. No appreciable differences in peak assignments in the FTIR profiles were found after 4 h of maturation at any of the Ca 2+ doping concentrations used (Supplementary Figure S1a–d). In parallel, Raman characterization (Figure 4b) show the most intense band at 996 cm −1 (ν 1 ), which can be assigned to the P–O symmetric stretching mode of PO 4 group in raphdophane-type orthophosphates, while that at ~1100 cm −1 is attributed to the antisymmetric stretching (ν 3 PO 4 ). The intensity of both bands decreases upon Ca 2+ doping. The region comprised between 300 and 700 cm −1 corresponds to the deformation modes of the PO 4 tetrahedron. The most intense band in this region is at 485 cm −1 and is assigned to the symmetric vibrations, while those at ~570 and 620 cm −1 can be ascribed to the asymmetric vibrations (ν 4 ) [38,39]. The presence of vaterite in the spectra for x = 0.05 and 0.07 M Ca 2+ , with bands at 1080–1090 cm −1 ν 1 CO 3 and 740–750 cm −1 ν 4 CO 3 [40] is hidden by the most intense bands of the phosphate groups. Clear differences were detected when plotting Raman spectra at increasing maturation times (Supplementary Figure S2). First, an increase in the intensity of the antisymmetric stretching mode ν 3 PO 4 at ~1100 cm −1 , and particularly in the less Ca 2+ -doped sample (Supplementary Figure S2a) is observed. Second, the highest Ca 2+ -doped sample shows the ν 1 PO 4 mode shifted from 970 cm −1 to 990 cm −1 (Supplementary Figure S2d), and the appearance of bands around 745 cm −1 and 1080 cm −1 (related to the vaterite phase). Also, the peaks at 845 cm −1 and 1460 cm −1 in samples at 4 and 24 h, in vibrational zones of citrate groups [41]. Thermogravimetric analyses (Supplementary Figure S3) revealed a behavior very close to the ones reported for lanthanide phosphate materials of raphdophane structure [29,42–45] but with some peculiarities reflecting the presence of citrates and carbonates in samples prepared at x = 0.05 and 0.07 M Ca 2+ . The first weight loss, recorded between T amb and 120–140 °C of about 2 wt%, is attributed to the residual adsorbed water, while the second one between 140 °C and about 600 °C, of 5–5.5 wt%, corresponds to the release of structural water, and this is the main weight loss. The third weight loss above 600 °C is associated with the decomposition of citrate molecules in samples prepared with x = 0.01 and 0.03 M Ca 2+ , and with decomposition of citrate and of CaCO 3 in CO 2 and CaO, when Figure 4. ( a ) FTIR and ( b ) Raman spectra of samples precipitated at 96 h using Ca 2+ -doping concentrations x= 0.01 M (purple), x= 0.03 M (green), x= 0.05 M (red), x= 0.07 M (light blue).
Nanomaterials 2021,11, 322 8 of 19 FTIR spectra of Ca 2+ -doped samples (Figure 4a) show basically the same spectroscopic features upon calcium doping, especially for x= 0.01, 0.03, and 0.05 M Ca 2+ . These are a broadband between 3600–3700 cm −1 and 2600 cm −1 corresponding to the O–H stretching of associated water, a main broad band at 1000–1100 cm −1 , which corresponds to the antisymmetric stretching mode of PO 43− groups ( ν3 PO 4 ) and two intense bands at ~620 and 535 cm −1 ascribed to the bending mode of the same PO 43− groups ( ν4 PO4). The broader signals around 1590–1620 cm −1 and 1405–1430 cm −1 are assignable to the antisymmetric and symmetric stretching frequencies of carboxylate ( − COO − ) groups of the adsorbed citrate [ 29 ]. No appreciable differences in peak assignments in the FTIR profiles were found after 4 h of maturation at any of the Ca 2+ doping concentrations used (Supplementary Figure S1a–d). In parallel, Raman characterization (Figure 4b) show the most intense band at 996 cm−1 ( ν1 ), which can be assigned to the P–O symmetric stretching mode of PO 4 group in raphdophane-type orthophosphates, while that at ~1100 cm −1 is attributed to the antisymmetric stretching ( ν3 PO 4 ). The intensity of both bands decreases upon Ca 2+ doping. The region comprised between 300 and 700 cm −1 corresponds to the deformation modes of the PO 4 tetrahedron. The most intense band in this region is at 485 cm −1 and is assigned to the symmetric vibrations, while those at ~570 and 620 cm −1 can be ascribed to the asymmetric vibrations (ν4) [38,39]. The presence of vaterite in the spectra for x= 0.05 and 0.07 M Ca 2+ , with bands at 1080–1090 cm −1ν1 CO 3 and 740–750 cm −1ν4 CO 3 [ 40 ] is hidden by the most intense bands of the phosphate groups. Clear differences were detected when plotting Raman spectra at increasing maturation times (Supplementary Figure S2). First, an increase in the intensity of the antisymmetric stretching mode ν3 PO 4 at ~1100 cm −1 , and particularly in the less Ca 2+ -doped sample (Supplementary Figure S2a) is observed. Second, the highest Ca 2+ -doped sample shows the ν1 PO 4 mode shifted from 970 cm −1 to 990 cm −1 (Supplementary Figure S2d), and the appearance of bands around 745 cm −1 and 1080 cm −1 (related to the vaterite phase). Also, the peaks at 845 cm −1 and 1460 cm −1 in samples at 4 and 24 h, in vibrational zones of citrate groups [41]. Thermogravimetric analyses (Supplementary Figure S3) revealed a behavior very close to the ones reported for lanthanide phosphate materials of raphdophane structure [29,42–45] but with some peculiarities reflecting the presence of citrates and carbonates in samples prepared at x= 0.05 and 0.07 M Ca 2+ . The first weight loss, recorded between T amb and 120–140 ◦ C of about 2 wt%, is attributed to the residual adsorbed water, while the second one between 140 ◦ C and about 600 ◦ C, of 5–5.5 wt%, corresponds to the release of structural water, and this is the main weight loss. The third weight loss above 600 ◦ C is associated with the decomposition of citrate molecules in samples prepared with x= 0.01 and 0.03 M Ca 2+ , and with decomposition of citrate and of CaCO 3 in CO 2 and CaO, when x= 0.05 and 0.07 M Ca 2+ . Specific losses are observed in these two samples. For x= 0.05 M Ca2+ the loss of CO2is around 0.6 wt% and for x= 0.07 M Ca2+ is of 2.2 wt%. Quantitative analyses of Ca, P, Tb, C, and H of as-prepared samples are reported in Table 1. This table also shows the percent weights of structural H 2 O determined by TGA and thus, the hydration number (n) of the raphdophane phase. Percent weights of CaCO 3 and citrate were determined by combining TGA data with mass balances. The data reveal increased percentages of dopant Ca from 0.42 wt% to 8.11 wt% in the structure of TbPO 4 .nH 2 O as the percentage of Tb decreases, according to the increase of Ca 2+ /Tb 3+ ratio in the precursor solutions. In these samples, the percentages of adsorbed citrate were around 1.1–1.2 wt% but in the highest Ca 2+ -doped sample that percentage rose to 4 wt%. This higher amount of citrate is likely due to the higher percentage of CaCO 3 , which can be also coated with citrate. Table 1also shows that structural H 2 O ranges between 5.0 and 6.3 wt% rendering hydration numbers around 0.9.
Nanomaterials 2021,11, 322 9 of 19 Table 1. Quantitative analyses of Ca, P, Tb, C, H, and estimated percent weights of structural citrate, H 2 O, CaCO 3 and hydration number n of the samples prepared with Ca 2+ doping concentration x ranging from 0.01 to 0.07 M, at 96 h. x[Ca2+] mol/L Ca (wt%) P (wt%) Tb (wt%) C (wt%) H (wt%) Cit (wt%) H2O str (wt%) CaCO3 (wt%) n 0.01 0.42 10.5 61.4 0.46 0.72 1.21 5.0 0 0.88 0.03 2.91 10.9 39.8 0.42 0.74 1.10 5.44 0.2 0.86 0.05 6.76, 6.09 * 12.0 27.5 0.52 0.75 1.12 6.68 0.76 0.93 0.07 10.32, 8.11 * 11.45 16.9 1.72 1.04 3.96 6.33 1.75 0.95 * wt% of dopant Ca in the TbPO4·nH2O structure. The analysis of CSD and ζ -potential versus pH of aqueous suspensions of the nanoparticles is also relevant to assess their potential as luminescent probes in nanomedicine applications. The tendency of the colloid to disperse or aggregate in simulated physiological conditions in the blood (pH around 7.4) or in the tumor microenvironment (pH around 5–6) are related to the size and surface charge of the nanoparticles [ 16 , 46 ]. In addition, these features have an impact on the formation of the protein corona around the nanoparticles [ 47 ]. In this study, the CSD of cit-Ca 2+ :TbPO 4· nH 2 O nanoparticles was plotted as cumulative volume-based distribution because they visually show the percentiles of the distribution D 10 , D 50 and D 90 (Figure 5and Supplementary Figure S4), widely employed to characterize crystal populations in pharmaceutical industry. These percentiles characterize the percentage of cumulative volume undersize distribution (percentage of the population smaller than the indicated size). Thus, D 10 is a percentile closer to the size of the individual particles while D 50 , the median of the population, is here somewhat influenced by particle aggregation. D 90 is entirely influenced by the aggregation of nanocrystals. The percentiles for samples prepared with x = 0.01, 0.03, 0.05, and 0.07 M Ca 2+ for 96 h were D 10 21, 51, 57, and 45 nm, respectively, and D50 37, 531, 122, and 94 nm, respectively (Figure 5b). In these samples, the evolution of cumulative CSD versus time (at 4 h, 24 h and 96 h, Figure S4a–d) does not follow a general trend, thus reflecting a difference in Ca composition as well as the presence of a secondary phase (vaterite) at high doping concentrations and its influence in the aggregation. These differences are also reflected in the profile of the ζ -potential versus pH curves (Figure 5c–f). While samples obtained with x= 0.01 and 0.03 M Ca 2+ displayed similar curves, with ζ -potential values − 17.3 and − 17.4 mV at pH 7, and − 14.0 and − 10.5 mV at pH 5 (Figure 5c,d), the curves of sample obtained with x= 0.05 M Ca 2+ (Figure 5e) and x= 0.07 M Ca 2+ (Figure 5f) show a different profile. The minimum ζ -potential values were found at pH 6.0 ( − 11.5 mV) and pH 8.0 ( − 15.9 mV) respectively. ζ -potentials were 0 beyond pH 6.0 in the first case, and below pH 8.0 in the second one. 3.2. Luminescence Properties of Cit-Ca2+:TbPO4·nH2O Nanoparticles 3.2.1. Luminescence in Solid-State It is well-known that some lanthanides, especially europium (III) and terbium (III), form highly fluorescent chelates with many different organic ligands. The sensitized fluorescence results from the ligand absorbing light, the energy of which is then transferred to the chelated metal ion. In fact, Tb(III) emits the energy as narrow-banded, line-type fluorescence with a long Stokes shift (over 250 nm) and an exceptionally long fluorescence decay time (up to 1 ms) [ 48 ]. Because of the long fluorescence decay time (over 10 times longer than the average background fluorescence) of Tb(III), a delay time (t d ) and a gate time (t g ) can be used during the measuring, remarkably reducing the background fluorescence.
Nanomaterials 2021,11, 322 16 of 19 lifetimes) and higher stability of their aqueous suspensions at the pH range of biological interest (5–7.4), are when using Ca 2+ doping concentration x= 0.01 M and x= 0.03 M, at any of the maturation times from 4 to 96 h. Summing up, the above properties are encouraging relative to the potential bioimaging applications of the nanocrystals. They can thus represent promising new luminescent nanoprobes for such applications and, if coupled with targeting and therapeutic moieties, they could be effective tools for theranostics. Supplementary Materials: The following are available online at https://www.mdpi.com/2079 -4991/11/2/322/s1, Figure S1: Evolution of FTIR spectra with time of samples prepared with different Ca 2+ doping concentrations x= 0.01 to 0.07 M, Figure S2: Evolution of Raman spectra with time of samples prepared with different Ca 2+ doping concentrations x= 0.01 to 0.07 M, Figure S3 : TGA analyses of precipitates obtained at 96 h from solutions with Ca 2+ doping concentrations ranging from (a) x= 0.01 to (d) x= 0.07 M, Figure S4: Cumulative volume oversize distribution of the cit-Ca 2+ :TbPO 4 .nH 2 O nanocrystals prepared with Ca 2+ doping concentrations x= 0.01, 0.03, 0.05 and 0.07 M at 4, 24 and 96 h, Figure S5: Excitation (dashed lines) and emission (solid lines) uncorrected spectra of solid cit-Ca 2+ :TbPO 4· nH 2 O samples prepared with x= 0.01 M Ca 2+ at maturation times of 96 h using td= 120 µs , t d = 5 ms and (a) λ exc/em = 230/545 nm, slit width exc/em = 2.5/2.5 nm , detector voltage 545 V; b) λ exc/em = 375/545 nm, slit width exc/em = 5/5 nm , detector voltage 470 v, Figure S6: Excitation (dashed lines) and emission (solid lines) uncorrected spectra of solid cit-Ca 2+ :TbPO 4· nH 2 O samples prepared with different Ca 2+ doped concentration at maturation times of 4 h, 24 h, 96 h and 7 days, Figure S7: Variation of the R.L.I. of the solid cit-Ca 2+ :TbPO 4· nH 2 O samples at the maximum excitation and emission wavelengths at several Ca 2+ concentrations when the maturation time is changed. Figure S8: Variation of the R.L.I. of the solid cit-Ca 2+ :TbPO 4· nH 2 O samples at the maximum excitation and emission wavelengths at several maturation time when the Ca 2+ concentration is changed. Figure S9: Luminescence decay curve of different solid cit-Ca 2+ :TbPO 4· nH 2 O samples at maturation times of 96 h, td= 100 µs , tg= 0.01 ms , λexc/em = 375/545 nm , slit-widths exc/em = 10/10 nm , and detector voltage = 600 V. Circles correspond to experimental data (100 cycles) and lines to the fitting equation. Figure S10: Variation of the luminescence lifetime of the solid cit-Ca 2+ :TbPO 4· nH 2 O nanoparticles prepared at several Ca 2+ concentrations when the maturation time is changed. Figure S11: Variation of the luminescence lifetime of the solid cit-Ca 2+ :TbPO 4· nH 2 O samples at several maturation times when the Ca 2+ concentration. Figure S12: Effect of the ionic strength over the (a) R.L.I. and (b) luminescence lifetime of the cit-Ca 2+ :TbPO 4· nH 2 O samples at 96 h maturation time dispersed in aqueous media at several Ca 2+ concentrations is changed. Figure S13. Effect of the temperature over the (a) R.L.I. and (b) luminescence lifetime of the cit-Ca 2+ :TbPO 4· nH 2 O samples at 96h maturation time dispersed in aqueous media at several Ca2+ concentrations. Author Contributions: Conceptualization, J.G.-M., D.C.-L., and M.P.; Investigation, J.G.-M., J.F.F.-S., M.P., I.R.-C., R.F.-P., A.D., and C.V.-E.; methodology, R.F.-P., A.D., J.F.F.-S., and C.V.-E; Supervision, J.G.-M.; writing—original draft preparation, J.G.-M. and M.P.; writing—review and editing, J.G.-M., M.P., and J.F.F.-S.; funding acquisition, J.G.-M., D.C.-L. and M.P. All authors have read and agreed to the published version of the manuscript. Funding: This research was funded by Spanish Agencia Estatal de Investigación of the Ministerio de Ciencia, Innovación y Universidades (MICIU) and co-funded with FEDER, UE, Project No. PGC2018- 102047-B-I00 (MCIU/AEI/FEDER, UE). J.F.F.-S. acknowledges the Spanish Ministerio de Economía y Competitividad Project No. CTQ2017-88079-P for support. M.P. acknowledges the Progetto di Ricerca Fondi di Ateneo per la Ricerca—FAR 2017 “Development of innovative biological materials for the functional regeneration of cardiac tissue models”. Acknowledgments: Authors acknowledge technical support of technician of the CIC of the University of Granada. Conflicts of Interest: The authors declare no conflict of interest.
Nanomaterials 2021,11, 322 17 of 19 References 1. Sreenivasan, V.K.A.; Zvyagin, A.V.; Goldys, E.M. Luminescent nanoparticles and their applications in the life sciences. J. Phys. Condens. Matter 2013,25, 194101. [CrossRef] [PubMed] 2. Li, J.; Zhu, J.-J. Quantum dots for fluorescent biosensing and bio-imaging applications. Analyst 2013 ,138, 2506. [CrossRef] [PubMed] 3. Fu, C.-C.; Lee, H.-Y.; Chen, K.; Lim, T.-S.; Wu, H.-Y.; Lin, P.-K.; Wei, P.K.; Tsao, P.H.; Chang, H.-C.; Fann, W. Characterization and application of single fluorescent nanodiamonds as cellular biomarkers. Proc. Natl. Acad. Sci. USA 2007 ,104, 727–732. [CrossRef] 4. Yeh, Y.-C.; Creran, B.; Rotello, V.M. Gold nanoparticles: Preparation, properties, and applications in bionanotechnology. Nanoscale 2012,4, 1871–1880. [CrossRef] 5. Wang, F.; Tan, W.B.; Zhang, Y.; Fan, X.P.; Wang, M.Q. Luminescent nanomaterials for biological labelling. Nanotechnology 2006 ,17, R1–R13. [CrossRef] 6. Oltolina, F.; Gregoletto, L.; Colangelo, D.; Gómez-Morales, J.; Delgado-López, J.M.; Prat, M. Monoclonal antibody-targeted fluorescein-5-isothiocyanate-labeled biomimetic nanoapatites: A promising fluorescent probe for imaging applications. Langmuir 2015,31, 1766–1775. [CrossRef] [PubMed] 7. Neacsu, I.A.; Stoica, A.E.; Vasile, B.S.; Andronescu, E. Luminescent hydroxyapatite doped with rare earth elements for biomedical applications. Nanomaterials 2019,9, 239. [CrossRef] 8. Gómez-Morales, J.; Verdugo-Escamilla, C.; Fernández-Penas, R.; Parra-Milla, C.M.; Drouet, C.; Maube-Bosc, F.; Oltolina, F.; Prat, M .; Fernández-Sánchez, J.F. Luminescent biomimetic citrate-coated europium-doped carbonated apatite nanoparticles for use in bioimaging: Physico-chemistry and cytocompatibility. RSC Adv. 2018,8, 2385–2397. [CrossRef] 9. Derfus, A.M.; Chan, W.C.W.; Bhatia, S.N. Probing the cytotoxicity of semiconductor quantum dots. Nano Lett. 2004 ,4, 11–18. [CrossRef] 10. Fang, Y.-P.; Xu, A.-W.; Song, R.-Q.; Zhang, H.-X.; You, L.-P.; Yu, J.C.; Liu, H.-Q. Systematic synthesis and characterization of single-crystal lanthanide orthophosphate nanowires. JACS 2003,125, 16025–16034. [CrossRef] 11. Luo, Q.; Shen, S.; Lu, G.; Xiao, X.; Mao, D.; Wang, Y. Synthesis of cubic ordered mesoporous YPO4:Ln 3+ and their photoluminescence properties. J. Mater. Chem. 2009,19, 8079–8085. [CrossRef] 12. Zhang, F.; Wong, S.S. Ambient large-scale template-mediated synthesis of high-aspect ratio single-crystalline, chemically doped rare-earth phosphate nanowires for bioimaging. ACS Nano 2010,4, 99–112. [CrossRef] [PubMed] 13. Di, W.; Li, J.; Shirahata, N.; Sakka, Y.; Willingere, M.-G.; Pinna, N. Photoluminescence, cytotoxicity and in vitro imaging of hexagonal terbium phosphate nanoparticles doped with europium. Nanoscale 2011,3, 1263–1269. [CrossRef] 14. Ito, H.; Fujishiro, Y.; Sato, T.; Okuwaki, A. Preparation of lanthanide orthophosphates by homogeneous precipitation under hydrothermal conditions using lanthanide-EDTA chelates. Br. Ceram. Trans. 1995,94, 146–150. 15. Zollfrank, C.; Scheel, H.; Brungs, S.; Greil, P. Europium(III) orthophosphates: Synthesis, characterization, and optical properties. Cryst. Growth Des. 2008,8, 766–770. [CrossRef] 16. Iafisco, M.; Delgado-López, J.M.; Varoni, E.M.; Tampieri, A.; Rimondini, L.; Gómez-Morales, J.; Prat, M. Cell surface receptor targeted biomimetic apatite nanocrystals for cancer therapy. Small 2013,9, 3834–3844. [CrossRef] 17. Iafisco, M.; Marchetti, M.; Gómez-Morales, J.; Hernández-Hernández, M.A.; García-Ruiz, J.M.; Roveri, N. Silica gel template for calcium phosphates crystallization. Cryst. Growth Des. 2009,9, 4912–4921. [CrossRef] 18. Ramírez-Rodríguez, G.B.; Delgado López, J.M.; Gómez-Morales, J. Evolution of calcium phosphate precipitation in hanging drop vapor diffusion by in situ Raman microspectroscopy. CrystEngComm 2013,15, 2206–2212. [CrossRef] 19. Bu, W.; Zhang, L.; Hua, Z.; Chen, H.; Shi, J. Synthesis and characterization of uniform spindle-shaped microarchitectures self-assembled from aligned single-crystalline nanowires of lanthanum phosphates. Cryst. Growth Des. 2007 ,7, 2305–2309. [CrossRef] 20. Fang, Y.-P.; Xu, A.-W.; Dong, W.-F. Highly improved green photoluminescence from CePO 4 :Tb/LaPO 4 core/shell nanowires. Small 2005,1, 967–971. [CrossRef] 21. Nuñez, N.O.; Liviano, S.R.; Ocaña, M.J. Citrate mediated synthesis of uniform monazite LnPO 4 (Ln = La, Ce) and Ln:LaPO 4 (Ln = Eu, Ce, Ce + Tb) spheres and their photoluminescence. Colloid Interface Sci. 2010,349, 484–491. [CrossRef] 22. Patra, C.R.; Bhattacharya, R.; Patra, S.; Basu, S.; Mukherjee, P.; Mukhopadhyay, D. Inorganic phosphate nanorods are a novel fluorescent label in cell biology. J. Nanobiotechnol. 2006,4, 11. [CrossRef] 23. Yu, C.; Yu, M.; Li, C.; Liu, X.; Yang, J.; Yang, P.; Lin, J. Facile sonochemical synthesis and photoluminescent properties of lanthanide orthophosphate nanoparticles. J. Solid State Chem. 2009,182, 339–342. [CrossRef] 24. Wang, X.; Gao, M. A facile route for preparing rhabdophane rare earth phosphate nanorods. J. Mater. Chem. 2006 ,16, 1360–1365. [CrossRef] 25. Hou, Z.; Wang, L.; Lian, H.; Chai, R.; Zhang, C.; Cheng, Z.; Lin, J. Preparation and luminescence properties of Ce 3+ and/or Tb 3+ doped LaPO4nanofibers and microbelts by electrospinning. J. Solid State Chem. 2009,182, 698–708. [CrossRef] 26. Xing, Y.; Li, M.; Davis, S.A.; Mann, S. Synthesis and characterization of cerium phosphate nanowires in microemulsion reaction media. J. Phys. Chem. B 2006,110, 1111–1113. [CrossRef] 27. Liu, X.; Wang, Q.; Gao, Z.; Sun, J.; Shen, J. Fabrication of lanthanide phosphate nanocrystals with well-controlled morphologies by layer-by-layer adsorption and reaction method at room temperature. Cryst. Growth Des. 2009,9, 3707–3713. [CrossRef]
Nanomaterials 2021,11, 322 18 of 19 28. Huong Tran, T.; Anh Tran, K.; Khuyen Hoang, T.; Hien Pham, T.; Minh Le, Q. Fabrication and properties of terbium phosphate nanorods. Adv. Nat. Sci. Nanosci. Nanotechnol. 2012,3, 015010. [CrossRef] 29. Gómez-Morales, J.; Verdugo-Escamilla, C.; Fernández-Penas, R.; Parra-Milla, C.M.; Drouet, C.; Iafisco, M.; Oltolina, F.; Prat, M.; Fernández-Sánchez, J.F. Bioinspired crystallization, sensitized luminescence and cytocompatibility of citrate-functionalized Ca-substituted europium phosphate monohydrate nanophosphors. J. Colloid Interface Sci. 2019,538, 174–186. [CrossRef] 30. López-Macipe, A.; Gómez-Morales, J.; Rodríguez-Clemente, R. Nanosized hydroxyapatite precipitation from homogeneous calcium/citrate/phosphate solutions using microwave and conventional heating. Adv. Mater. 1998,10, 49–53. [CrossRef] 31. Delgado-López, J.M.; Iafisco, M.; Rodríguez, I.; Prat, M.; Gómez-Morales, J.; Tampieri, A. Crystallization of bioinspired citratefunctionalized nanoapatites with tailored carbonate content. Acta Biomater. 2012,8, 3491–3499. [CrossRef] 32. Martínez-Casado, F.J.; Iafisco, M.; Delgado-López, J.M.; Martínez-Benito, C.; Ruiz-Pérez, C.; Colangelo, D.; Oltolina, F.; Prat, M.; Gómez-Morales, J. Bioinspired citrate–apatite nanocrystals doped with divalent transition metal ions. Cryst. Growth Des. 2016 ,1, 145–153. [CrossRef] 33. Delgado-López, J.M.; Frison, R.; Cervellino, A.; Gómez-Morales, J.; Guagliardi, A.; Masciocchi, N. Crystal size, morphology, and growth mechanism in bio-inspired apatite nanocrystals. Adv. Funct. Mater. 2014,24, 1090–1099. [CrossRef] 34. Hu, Y.Y.; Rawal, A.; Schmidt-Rohr, K. Strongly bound citrate stabilizes the apatite nanocrystals in bone. Proc. Natl. Acad. Sci. USA 2010,107, 22425–22429. [CrossRef] 35. Coelho, A.A. TOPAS and TOPAS-Academic: An optimization program integrating computer algebra and crystallographic objects written in C++. J. Appl. Cryst. 2018,51, 210–218. [CrossRef] 36. Combes, C.; Bareille, R.; Rey, C. Calcium carbonate–calcium phosphate mixed cement compositions for bone reconstruction. J. Biomed. Mater. Res. Part A 2006,79, 318–328. [CrossRef] 37. Young, R.A. Introduction to the Rietveld method. In The Rietveld Method; Young, R.A., Ed.; Oxford University Press: Oxford, UK, 1993; pp. 1–38. 38. Clavier, N.; del Mesbah, A.; Szenknect, S.; Dacheux, N. Monazite, rhabdophane, xenotime & churchite: Vibrational spectroscopy of gadolinium phosphate polymorphs. Spectrochim. Acta Part A Mol. Biomol. Spectrosc. 2018,205, 85–94. [CrossRef] 39. Assaaoudi, H.; Ennaciri, A.; Rulmont, A. Vibrational spectra of hydrated rare earth orthophosphates. Vibrat. Spectr. 2001 ,2, 81–90. [CrossRef] 40. Donnelly, F.C.; Purcell-Milton, F.; Framont, V.; Cleary, O.; Dunne, P.W.; Gun’k, Y.K. Synthesis of CaCO 3 nano- and micro-particles by dry ice carbonation. Chem. Commun. 2017,53, 6657–6660. [CrossRef] [PubMed] 41. Tada, H.; Bronkema, J.L.; Bell, A. Application of in situ surface-enhanced Raman spectroscopy (SERS) to the study of citrate oxidation on silica-supported silver nanoparticles. Catal. Lett. 2004,92, 93–99. [CrossRef] 42. Lucas, S.; Champion, E.; Bernache-Assollant, D.; Leroy, G. Rare earth phosphate powders RePO 4· nH 2 O (Re = La, Ce or Y) II. Thermal behavior. J. Solid State Chem. 2004,177, 312–1320. [CrossRef] 43. Cho, J.; Kim, C.H. Solid-state phase transformation mechanism from hexagonal GdPO 4 :Eu 3+ nanorods to monoclinic nanoparticles. RSC Adv. 2014,4, 31385–31392. [CrossRef] 44. Kijkowska, R. Thermal decomposition of lanthanide orthophosphates synthesized through crystallisation from phosphoric acid solution. Thermochim. Acta 2003,404, 81–88. [CrossRef] 45. Colomer, M.T.; Delgado, I.; Ortiz, A.L.; Fariñas, J.C. Microwave-assisted hydrothermal synthesis of single-crystal nanorods of rhabdophane-type Sr-doped LaPO4.nH2O. J. Am. Ceram. Soc. 2014,97, 750–758. [CrossRef] 46. Jabalera, Y.; Oltolina, F.; Prat, M.; Jimenez-Lopez, C.; Fernández-Sánchez, J.F.; Choquesillo-Lazarte, D.; Gómez-Morales, J. Eu- Doped Citrate-Coated Carbonated Apatite Luminescent Nanoprobes for Drug Delivery. Nanomaterials 2020,10, 199. [CrossRef] 47. Lundqvist, V.; Stigler, J.; Elia, G.; Lynch, I.; Cedervall, T.; Dawson, K.A. Nanoparticle size and surface properties determine the protein corona with possible implications for biological impacts. Proc. Natl. Acad. Sci. USA 2008,105, 14265–14270. [CrossRef] 48. Hemmilä, I.; Dakubu, S.; Mukkala, V.-M.; Siitari, H.; Lövgren, T. Europium as a label in time-resolved immunofluorometric assays. Anal. Biochem. 1984,137, 335. [CrossRef] 49. Siqueira, K.P.F.; Lima, P.P.; Ferreira, R.A.S.; Carlos, L.D.; Bittar, E.M.; Matinaga, F.M.; Paniago, R.; Krambrock, K.; Moreira, R.L.; Dias, A.J. Influence of the Matrix on the Red Emission in Europium Self-Activated Orthoceramics. Phys. Chem. C 2015 ,119, 17825. [CrossRef] 50. Siqueira, K.P.F.; Lima, P.P.; Ferreira, R.A.S.; Carlos, L.D.; Bittar, E.M.; Granado, E.; González, J.C.; Abelenda, A.; Moreira, R.L.; Dias, A. Lanthanide Orthoantimonate Light Emitters: Structural, Vibrational, and Optical Properties. Chem. Mater. 2014 ,26, 6351. [CrossRef] 51. Medina-Velazquez, D.Y.; Caldiño, U.; Morales-Ramirez, A.; Reyes-Miranda, J.; López, R.E.; Escudero, R.; Ruiz-Guerrero, R.; Morales Perez, M.F. Synthesis of luminescent terbium-thenoyltriflouroacetone MOF nanorods for green laser application. Opt. Mater. 2019,87, 3–10. [CrossRef] 52. Richardson, F.S. Terbium(III) and europium(III) ions as luminescent probes and stains for biomolecular systems. Chem. Rev. 1982 , 82, 541. [CrossRef] 53. Guilbault, G.G. General Aspects of Luminescence Spectroscopy, Practical Fluorescence; Guilbault, G.G., Ed.; Marcel Dekker: New York, NY, USA, 1990. 54. ISO 10993-5 Biological Evaluation of Medical Devices Part 5: Tests for In Vitro Cytotoxicity; International Standard Organization: Geneva, Switzerland, 2009.
Nanomaterials 2021,11, 322 19 of 19 55. López-Macipe, A.; Gómez-Morales, J.; Rodriguez-Clemente, R. The role of pH in the adsorption of citrate ions on hydroxyapatite. J. Colloid Interface Sci. 1998,200, 114–120. [CrossRef] 56. Borroni, E.; Miola, M.; Ferraris, S.; Ricci, G.; Žužek Rožman, K.; Kostevšek, N.; Catizone, A.; Rimondini, L.; Prat, M.; Verné, E.; et al . Tumor targeting by lentiviral vectors combined with magnetic nanoparticles in mice. Acta Biomater. 2017 ,59, 303–316. [CrossRef] [PubMed] 57. Mooney, C.L. X-ray diffraction study of cerium phosphate and related crystals. I. Hexagonal modification. Acta Cryst. 1950 ,3, 337–340. [CrossRef]