scieee AI-readable full text Open interactive document viewer

Synthesis and characterization of magnetic chitosan microspheres as low-density and low-biotoxicity adsorbents for lake restoration

Vicente Álvarez De Manzaneda, María Inmaculada De,Funes, Ana Inmaculada,Vicente Álvarez-Manzaneda, Juan De

Abstract

The authors would like to thank F. Galisteo-Gonz alez for providing the Bool2k software used for the generation of particlesize distributions from SEM micrographs and F. Vereda for his help in the Chemistry Laboratory. This workwas supported by Junta de Andalucía projects of excellence P10-RNM-6630 and P11-FQM- 7074 (Spain); MINECO CTM 2013-46951-R, MAT 2013-44429-R and PCIN 2015-051, MAT 2016-78778-R projects (Spain); and by the European Regional Development Fund.

Full text

1 Title: Synthesis and characterization of magnetic chitosan microspheres as low-density 1 and low-biotoxicity adsorbents for lake restoration 2 Authors: A. Funesa,b*, J. de Vicentec and I. de Vicentea,b 3 Affiliations: (a) Departamento de Ecología, Facultad de Ciencias, Universidad de Gra-4 nada, 18071 Spain 5 (b) Instituto del Agua, Universidad de Granada, 18071 Spain 6 (c) Departamento de Física Aplicada, Facultad de Ciencias, Universidad de Granada, 7 18071 Spain 8 9 Full address for correspondence: 10 * Corresponding author. 11 Departamento de Ecología, Facultad de Ciencias, Universidad de Granada, 18071 Spain 12 Phone: (+34) 958 248323; Fax: (+34) 958 243093 ; email: [email protected] 13 14 Keywords: magnetite, magnetic chitosan, emulsion, phosphorus, eutrophication15 2 Abstract 16 We propose a novel magnetic adsorbent for optimal Phosphorus (P) removal from the 17 upper sediment layers. For this aim, magnetic chitosan microparticles were prepared 18 using a reverse-phase suspension cross-linking technique. The resulting particles and 19 suspensions were characterized using scanning electron microscopy, X-ray powder dif-20 fraction, Fourier transform infrared spectroscopy, magnetometry, thermogravimetric 21 analysis, electrophoretic mobility and turbidity measurements. The hybrids are multi-22 core particles consisting of well dispersed magnetite nanoparticles (approx. 10 % w/w) 23 homogeneously distributed within the biopolymer matrix. These microparticles can be 24 easily separated from the water column and sediment using magnetic field gradients. 25 Their P adsorption capacity is evaluated in batch conditions resulting in a maximum P 26 adsorption capacity of = 4.84 mg g-1 at pH = 7. We demonstrate that these particles 27 are excellent candidates to remove P from water column and also P mobile from the 28 upper sediment layers due to two main reasons: they sediment slower and present lower 29 potential toxicity (due to a their larger size) than conventional iron/iron oxide micropar-30 ticles previously proposed for lake restoration. 31 3 1. Introduction 32 Enrichment of phosphorus (P) is considered the main cause of eutrophication of inland 33 waters (Carpenter, 2005). In situations in which P release from sediment (internal P 34 load) impedes lake recovery once external P load has been reduced, in-lake addition of 35 P-binding adsorbents appears as an advisable alternative for lake management (Cooke et 36 al., 2005; Søndergaard et al., 2003). Z2G1 or Aqual-P®, Phoslock®, calcium, iron (Fe) 37 or alum salts have been demonstrated to increase sediment P-sorption capacity (Cooke 38 et al., 2005; Dittrich et al., 2011; Gibbs et al., 2011; Robb et al., 2003; Søndergaard et 39 al., 2003). Although some of these techniques could represent a long-lasting sink for P, 40 changes in physicochemical conditions or resuspension events can lead to undesirable P 41 release to water column along with toxic substances stemming from the adsorbents 42 composition (Egemose et al., 2009; Zamparas and Zacharias, 2014). 43 In the last decades, magnetic nano- and microparticles have attracted special attention to 44 adsorb contaminants from waters and soils due to their easy separation and recovery 45 from the medium for further reuse. This obviously leads to cost savings and to the re-46 duction of the contact time with biota (Crane and Scott, 2012; Gómez-Pastora et al., 47 2014; Huber, 2005; Lu et al., 2007; Tang and Lo, 2013). With this in mind, more re-48 cently, these magnetic particles have been successfully used for P removal in the con-49 text of lake restoration and improvement of water quality (Choi et al., 2016; Daou et al., 50 2007; de Bashan and Bashan, 2004; de Vicente et al., 2010; Funes et al., 2016, 2014; 51 Lai et al., 2016; Long et al., 2011; Shaikh and Dixit, 1992). 52 Apart from high P adsorption capacity and reusability, magnetic particles must meet 53 other stringent requirements for lake restoration applications. Particle size has very im-54 portant implications not only in adsorption capacity but also in biological toxicity. 55 4 Small (nano) particles are preferred to enhance adsorption capacity (because of their 56 large surface area) (Yavuz et al., 2006). However, there are evidences of toxicological 57 effects on aquatic organisms (Oberdörster, 2004); because cladocerans such as Daphnia 58 sp. filter large volumes of water, considerable amounts of nanoparticles can be ingested 59 by them, having negative consequences in their physiology and also in upper levels of 60 the food chain (Lovern and Klaper, 2006, Zhu et al., 2010). Unfortunately, nanoparticles 61 can also negatively affect aquatic biota by adsorption on their carapaces and filtrations 62 apparatus (Baumann et al., 2014). Finally, Fe dissolution is another indirect effect of 63 using Fe based nanoparticles which can led to phytotoxicity (Keller et al., 2012). 64 Of outstanding importance in this work is particle density. Actually, particle density is a 65 key factor driving adsorbent distribution through the sediment profile and determines its 66 availability for P adsorption. It is worth to stress here that sedimentary P mobile, which 67 is the target P pool, mostly concentrates within the first 10 cm of sediment and de-68 creases rapidly with depth (Reitzel et al., 2005). From this perspective, very large den-69 sity particles are not desirable because they sink deeper in sediment being not available 70 for P adsorption. Moreover, sinking of magnetic particles into deeper layers may con-71 tribute to intense sediment resuspension when removing the magnetic particles with the 72 magnet causing undesirable effects (Søndergaard et al., 1992). In addition, large density 73 particles may sink into the deepest sediment layers where magnetophoretic forces ex-74 erted by the magnets could not be large enough to overcome opposing surface (cohe-75 sive) forces within the sediment making the recovery process inefficient (Yavuz et al., 76 2006). Thus, a balance between high P removal efficiency (high affinity and large sur-77 face area), low bio-toxicity (biocompatible components and large particle size to diffi-78 cult the ingestion by biota) and low density (to remain in the first 10 cm of sediment) 79 must be pursued (Philippova et al., 2011; Reddy and Lee, 2013). 80 5 In this work, we fabricate hybrid magnetic particles (magnetic chitosan microspheres, 81 MCMs) that accomplish the three requirements discussed in paragraph above. We fol-82 low a novel approach that consists in the encapsulation of magnetic multicores within a 83 biopolymer spherical matrix that prevents Fe dissolution, is non-toxic and less dense 84 (than traditional magnetic adsorbents), but still exhibiting a large adsorption capacity 85 for lake restoration applications. Furthermore, by using a chitosan matrix we introduce 86 versatile adsorption properties (apart from the traditional specific adsorption mechanism 87 between P and Fe oxides) that can be controlled through the cross-linker concentration 88 due to the presence of amine and hydroxyl groups and therefore pH dependent electro-89 static interactions. 90 2. Materials and Methods 91 All reagents were of analytical grade and used without further purification. FeCl3·6H2O, 92 ethylene glycol (EG) and sodium acetate (NaAc) were supplied from VWR (AnalaR-93 Normapur). Trisodium citrate (Na3Cit) was obtained from Carlo Erba. Chitosan (low 94 molecular weight; 75-80 % deacetylated), glutaraldehyde (8%), mineral oil, Span 80 95 and petroleum ether were acquired from Sigma Aldrich. Acetic acid (5%) and acetone 96 were obtained from Panreac. Finally, carbonyl Fe microparticles were obtained from 97 BASF (grade HQ, average diameter = 800 nm, Germany). 98 2.1 Synthesis of magnetite (Fe3O4) nanoparticles 99 There are several routes for the synthesis of Fe3O4 depending on the particle size to be 100 obtained. For instance, Fe3O4 nanoparticles of typical sizes in the range  10 nm can be 101 prepared by the Massart's method (Massart, 1981). In this case, Fe+2 and Fe+3 are 102 coprecipitated in an alkaline solution. Another option to obtain Fe3O4 particles in the 103 6 micronsized range,  1000 nm, is to follow Sugimoto and Matijevic (1980). In this case, 104 Fe+2 oxidation is slowed down by a nitrate salt allowing the particles to grow larger. In 105 this particular work, we are interested in particles having an intermediate particle size ( 106 100 nm): large enough to respond to magnetophoretic forces and small enough for a 107 large surface activity and hence adsorption capacity. 108 We used a solvothermal method following the recommendations by Liu et al. (2009a) 109 with slight modifications. Briefly, 3.38 g of FeCl3·6H2O (0.25 mol L-1) and 0.5 g of 110 Na3Cit (34 mmol L-1) were dissolved in 50 mL of ethylene glycol by using a centrifugal 111 mixer (3 min at 1000 rpm). NaAc (3 g) was then added and the suspension was mixed 112 again (15 min at 1000 rpm). Next, the mixture was sealed in a Teflon-lined stainless-113 steel autoclave (125 mL capacity) and heated at 215 ºC for 10 h. The obtained magnetic 114 nanoparticles were washed several times with ethanol and dried at 50 ºC for 4 hours. 115 2.2 Preparation of magnetic chitosan microspheres (MCMs) 116 MCMs where fabricated by a reverse-phase suspension cross-linking technique follow-117 ing Jiang et al. (2005) with slight modifications. First, previously synthesized Fe3O4 118 powder (0.082 g) was dispersed via ultrasonication in a solution of chitosan (0.25 g) in 119 5% acetic acid (10 mL) for 10 min. The Fe3O4:chitosan ratio (by weight) was 1:3. Next, 120 10 mL of this suspension were added drop-wise to a mixture of mineral oil (37.5 mL) 121 and Span 80 (2.5 g) as a surfactant. During all the process, the formed emulsion was 122 stirred with a mechanical stirrer at 2500 rpm for 30 min. Then, 5 mL of glutaraldehyde 123 were added dropwise and the dispersion was stirred for another 1 h at 40 ºC to promote 124 the cross-linking. Finally, the magnetic microspheres were separated from the oil phase 125 by applying a magnet for 30 min and washed several times with petroleum ether and 126 acetone. MCMs were then dried at 50 ºC for 4 h and stored until use. Chitosan micro-127 7 spheres (CMs) were prepared following the same procedure as MCMs without addition 128 of Fe3O4. CMs were separated from oil phase by centrifugation at 3000 rpm for 5 min, 129 washed and stored as in MCMs procedure. 130 2.3 Characterization of the hybrid particles 131 Size and surface morphology of Fe3O4, MCMs and CMs particles were elucidated with 132 high-resolution field-emission scanning electron microscopy (FIB-FESEM, AURIGA, 133 Carl Zeiss SMT Inc.). Environmental scanning electron microscopy (ESEM, FEI 134 Quanta 400) was used to determine internal distribution of Fe3O4 particles within 135 MCMs. Samples were embedded within an Epofix resin and cross-sectioned. Crystal 136 structure of Fe3O4 and MCMs was analyzed with a Bruker D8 Advance X-Ray difrac-137 tometer (XRD) with scattering angle (2θ) of 0-90º using Cu-Kα as incident radiation ( 138 = 0.1540 Å) at 40 kV. Fourier transform infrared spectroscopy (FT-IR) was recorded 139 between 4000-400 cm-1 on a JASCO 6200 spectrophotometer in attenuated total reflec-140 tion (ATR) mode to observe interactions between functional groups of the different syn-141 thesized systems. Samples were prepared with KBr disks. Thermal stability of the dif-142 ferent composites was analyzed by a thermogravimetric analyzer (METTLER TOLEDO 143 mod.DCS1). Samples were heated from 37 to 950 ºC with a heating rate of 10 ºC min-1 144 in N2 atmosphere. The magnetization measurements of the composites were performed 145 with a SQUID magnetometer (MPMS XL, Quantum Desing) at room temperature. The 146 external field was swept from -4000 to 4000 kA m-1. Electrophoretic mobility of the 147 composites was determined using a Zetasizer Nano Z (Malvern instruments, UK) at 25 148 ºC. To minimize sedimentation of magnetic particles under gravity, prior to the test, the 149 samples were sonicated for 5 min. Samples for measuring electrophoretic mobility were 150 prepared as follows: a suspension of Fe3O4 (0.1 g L-1) or MCMs (0.72 gL-1) or CMs 151 8 (0.62 g L-1) with 3 mM NaHCO3 was agitated for 24 h in a horizontal shaker (150 rpm) 152 at different pH values. Afterwards, pH was readjusted and the suspensions were made 153 up to 25 mL of volume. Turbidity measurements were performed using a Turbiscan MA 154 2000 (Formulaction, France) in order to compare sedimentation rates of MCMs and 155 carbonyl Fe microparticles used by de Vicente et al. (2010). Briefly, dispersions were 156 placed in a cylindrical plastic cell which was scanned from the bottom to the top with an 157 incident near infrared light source (air = 850 nm; Wulff-Pérez et al., 2009). Measure-158 ments reported here only consider transmission data -as a function of sample height and 159 time-. Samples were prepared by mixing a suspension of carbonyl Fe microparticles 160 (0.1 g L-1) or MCMs (0.72 g L-1) with 3 mM NaHCO3 under agitation for 24 h at pH 7 161 in a final volume of 25 mL. 162 2.4 Batch adsorption experiments 163 Fe3O4, MCMs and CMs stock suspensions were prepared by mixing either 100 mg or 164 720 mg or 620 mg, respectively, with 100 mL of distilled water in a polyethylene con-165 tainer. Suspensions were sonicated for 5 min prior to their use for adsorption experi-166 ments to ensure homogeneity of the dispersion. As 2.5 mL of the stock solution (1 g 167 Fe3O4 L-1; 7.2 g MCMs L-1; 6.2 g CMs L-1) were added to a final volume of 25 mL, the 168 final concentration for each suspension was 0.1 g Fe3O4 L-1, 0.72 g MCMs L-1 and 0.62 169 g CMs L-1. 170 To investigate the effect of pH on P removal efficiency by MCMs, 2.5 mL of a MCMs 171 stock suspension (7.2 g L-1) were mixed with 20 mL of 3 mM NaHCO3 (acting as a 172 buffer) and shaked for 24 h in a horizontal shaker (150 rpm). Then, 2 mL of a 0.125 173 mM P stock solution were added to each tube and pH was adjusted to 7, 8 and 9. Sus-174 pensions were shaked (150 rpm) for 24 h. After this time, pH was readjusted and the 175 9 volume was made up to 25 mL with 3 mM NaHCO3. Initial P concentration accounted 176 for 0.01 mM P. A magnetic separation gradient (PASCO scientific; EM-8641) was ap-177 plied for 5 min and the supernatant was filtered to measure P by spectrophotometric 178 procedure according to Murphy and Riley (1962). 179 Maximum P adsorption capacity was tested by adding 2.5 mL of the corresponding 180 stock suspension to 20 mL 3 mM NaHCO3 in 25 mL centrifuge tubes. Final adsorbent 181 concentrations of Fe3O4 and CMs isotherms were fixed according to Fe3O4 and chitosan 182 content in MCMs as obtained from magnetometry tests. Suspensions were shaked (150 183 rpm) for 24 h and then, 2 mL of KH2PO4 solutions with P concentrations ranging from 184 0.125 to 2 mM P were added. The pH value was adjusted to 7 and suspensions were 185 shaked again (150 rpm) for 24 h. Afterwards, pH was readjusted and the volume was 186 made up to 25 mL with 3 mM NaHCO3. The magnetic separation gradient was applied 187 for 5 min and P determination was carried out as previously mentioned. The equilibrium 188 adsorption capacity of P, , was calculated as follows: 189 [1] 190 where C0 and are the initial and equilibrium P concentration (mg L-1), respectively, 191 is the mass of adsorbent in grams and is the total volume of the suspension (L). 192 3. Results and discussion 193 3.1 Characterization of composites 194 Fig. S1 (supplemental material) shows a typical SEM image of the Fe3O4 particles. As 195 observed, they are quasi-spherical in shape and uniform in size with a mean diameter of 196 about 280 nm. A detailed description of their morphological characteristics is provided 197 16 sorption increased when increasing concentration but tended to reach a constant value at 340 higher phosphate concentrations in accordance to the model (Biswas et al., 2008) . Al-341 though the same adsorption mechanism could be applied to Fe3O4, the saturation value 342 was reached very quickly compared to MCMs and CMs (Fig. 5). Table 1 shows the best 343 fitting parameters for Fe3O4, MCMs and CMs, and the corresponding correlation coeffi-344 cients. Note that for comparative purposes, in these experiments, the magnetite concen-345 tration was the same (constant) in Fe3O4 and MCMs suspensions. Also, the chitosan 346 concentration in CMs and MCMs suspensions was kept the same. The highest maxi-347 mum P adsorption capacity ( ) was reported by MCMs (4.84 mg g-1) followed by 348 CMs (2.41 mg g-1) and Fe3O4 (2.27 mg g-1). Table 1 also summarizes maximum P ad-349 sorption capacities of different adsorbents of interest found in the literature. P adsorp-350 tion capacity values of Phoslock® (Haghseresht, 2005; Zamparas et al., 2012), alum (de 351 Vicente et al., 2008) or some clays such as Zenit/Fe (Zamparas et al., 2012) and clinop-352 tilolite (Sakadevan and Bavor, 1998) are closer to values obtained for MCMs. On the 353 contrary, synthetic zeolite HUD (Onyango et al., 2007) and CFH-12 (Lyngsie et al., 354 2014) present much higher P sorption capacities compared to MCMs. Isotherm data 355 pointed out a P removal efficiency by MCMs higher than 45 % for concentrations rang-356 ing from 10 to 160 µmol P L-1 when using a concentration of 0.72 g MCMs L-1. Then, it 357 can be stated that MCMs would be potentially able to remove 60 % of P from water 358 column of hypertrophic water bodies whose average water column TP have been deter-359 mined to be higher than 100 µg L-1 (3.23 µmol P L-1) (Nürnberg, 1996). 360 Differences in P adsorption capacity of Fe3O4, MCMs and CMs can be explained by the 361 different surface characteristics of the systems. The low P adsorption capacity found for 362 Fe3O4 is in the range of that found by Daou et al. (2007) (although at a different pH 363 value; pH = 3) who reported a maximum P adsorption capacity of 5.2 mg P g-1 (Table 1) 364 17 when using a positively charged Fe3O4 with higher surface area (40 nm average particle 365 size). However, a much higher P adsorption capacity is also reported in the literature for 366 the same pH conditions to our study. de Vicente et al. (2010) found that negatively 367 charged Fe3O4 (90 nm) was able to adsorb a maximum of 27.15 mg P g-1 (Table 1). At 368 pH = 7, our Fe3O4 exhibits a negative surface charge (electrophoretic mobility -2.7 ± 369 0.45 µm cm V-1 s-1) which suggests that P adsorption mechanism is driven by specific 370 interactions (and not by electrostatic interactions). The comparatively low P adsorption 371 capacity found in our Fe3O4 is explained by the organic layer (supported by TGA and 372 FT-IR analysis) covering Fe3O4 surface that may difficult P adsorption onto hydroxyl 373 functional groups present on its surface (Antelo et al., 2005; Sun et al., 1998). 374 CMs adsorption capacity reported in this work is low compared to other studies employ-375 ing cross-linked chitosan composites with the same pH conditions as the cases of Filip-376 kowska et al. (2014) and Sowmya and Meenakshi (2014) who reported a P maximum 377 adsorption capacity of 58.5 mg g-1and 108.2 mg g-1, respectively (Table 1). Synthesized 378 CMs showed a slight negative surface charge as indicated by electrophoretic mobility (-379 0.84 ± 0.65 µm cm V-1 s-1) similarly to other cross-linked chitosan composites (Yao et 380 al., 2014). Indeed, the point of zero charge (pzc) for most chitosan particles has been 381 previously reported to range between 6.2 and 6.7 (Chatterjee et al., 2005; Elwakeel, 382 2009). P adsorption onto CMs is thought to be due to physical adsorption or intraparti-383 cle diffusion through the chains network of the particle (Crini and Badot, 2008). 384 It is noteworthy that MCMs are positively charged despite of the fact that Fe3O4 and 385 CMs are negatively charged at pH = 7. This is expected because the embedded magnet-386 ite grains interfere in the cross-linking process. The reason is that chitosan surface 387 charge is determined by protonation/deprotonation of its surface functional groups 388 18 (amine and hydroxyl groups) depending on pH (Pillai et al., 2009; Reddy and Lee, 389 2013). During the synthesis process in acidic media, aldehyde groups of glutaraldehyde 390 mainly react with protonated amine and hydroxyl groups (Crini and Badot, 2008). As 391 suggested in previous works, a higher extent of cross-linking reduces particle size and 392 surface zeta potential due to condensation of polymer chains and reduction of positively 393 charged free amino groups, respectively (Crini and Badot, 2008; He et al., 1999; Rodri-394 gues et al., 2012). In our case, the larger particle size of MCMs (compared to CMs) 395 suggests a lower degree of cross-linking that is expected and attributed to the physical 396 interference of magnetite in the Schiff´s base reaction giving a net positive charge to the 397 hybrid particles. 398 Reuse of MCMs is essential for their practical use and cost effectiveness. In this con-399 text, a conventional protocol that works well in the case of iron oxides consists in wash-400 ing the particles with a concentrated NaOH solution. With this in mind, after a typical 401 adsorption experiment, the MCMs particles were washed twice with 1M NaOH and 3 402 times with 3 mM NaHCO3 using magnetic separation. This particular protocol although 403 successful for magnetite and carbonyl Fe particles (de Vicente et al., 2010) failed in the 404 case of MCMs (the P adsorption capacity of reused particles was very low). Degrada-405 tion of the adsorbent may be another important issue for practical applications. How-406 ever, chitosan solubilisation is not likely to occur in natural environments because 407 strong acidic conditions are required (Crini and Badot, 2008). Nevertheless, the cross-408 linking level in MCMs may definitely have an effect and its impact in the resulting 409 chemical stability and mechanical resistance of the microparticles are open issues for 410 future work. 411 4. Conclusions 412 19 We propose a novel magnetic adsorbent for P removal from the upper sediment layers. 413 It consists on very low density hybrid multigrain microparticles prepared by a reverse-414 phase suspension cross-linking technique. The microparticles are constituted by well 415 dispersed magnetite nanocores within a spherical chitosan microparticle (approx. 10 % 416 w/w) that is biocompatible and non toxic. These particles do exhibit a sufficient P ad-417 sorption capacity ( = 4.84 mg g-1) to be used in eutrophic systems at conventional pH 418 levels. The mechanism behind the adsorption is dual: electrostatic for the case of chito-419 san matrix and surface specific for the case of magnetite grains. This provides versatile 420 adsorption properties toward cation species as well. Because of their large size and 421 magnetite loading, these hybrid microparticles can be easily separated using magneto-422 phoresis. 423 Apart from their versatile adsorption properties, the major advantage of these particles 424 is that, once settled from the water column, they have the ability to remain in the upper 425 layers of the sediment where the target sedimentary P pool in eutrophic lakes (P mobile) 426 concentrates. This is due to their much lower particle density compared to other mag-427 netic adsorbents previously proposed for lake restoration. Another interesting aspect of 428 the synthesized microparticles is the low toxicity for aquatic biota due to their high par-429 ticle size. Further investigation about MCMs reutilization is still needed in order to 430 make these particles cost-effective as P adsorbents. 431 Acknowledgments 432 The authors would like to thank F. Galisteo-González for providing the Bool2k software 433 used for the generation of particle-size distributions from SEM micrographs and F. 434 Vereda for his help in the Chemistry Laboratory. This work was supported by Junta de 435 Andalucía projects of excellence P10-RNM-6630 and P11-FQM-7074 (Spain); 436 20 MINECO CTM 2013-46951-R, MAT 2013-44429-R and PCIN 2015-051, MAT 2016-437 78778-R projects (Spain); and by the European Regional Development Fund (ERDF). 438 21 References Agnihotri, S.A., Aminabhavi, T.M., 2004. Controlled release of clozapine through chitosan microparticles prepared by a novel method. J. Control. Release 96, 245–259. doi:10.1016/j.jconrel.2004.01.025. Antelo, J., Avena, M., Fiol, S., López, R., Arce, F., 2005. Effects of pH and ionic strength on the adsorption of phosphate and arsenate at the goethite-water interface. J. Colloid Interface Sci. 285, 476–486. doi:10.1016/j.jcis.2004.12.032. Baumann, J., Köser, J., Arndt, D., Filser, J., 2014. The coating makes the difference: Acute effects of iron oxide nanoparticles on Daphnia magna. Sci. Total Environ. 484, 176–184. doi:10.1016/j.scitotenv.2014.03.023. Biswas, B.K., Inoue, K., Ghimire, K.N., Harada, H., Ohto, K., Kawakita, H., 2008. Removal and recovery of phosphorus from water by means of adsorption onto orange waste gel loaded with zirconium. Bioresour. Technol. 99, 8685–8690. doi:10.1016/j.biortech.2008.04.015. Cai, W., Wan, J., 2007. Facile synthesis of superparamagnetic magnetite nanoparticles in liquid polyols. J. Colloid Interface Sci. 305, 366–370. doi:10.1016/j.jcis.2006.10.023 Carpenter, S.R., 2005. Eutrophication of aquatic ecosystems: bistability and soil phosphorus. Proc. Natl. Acad. Sci. U. S. A. 102, 10002–10005. doi:10.1073/pnas.0503959102. Chatterjee, S., Chatterjee, S., Chatterjee, B.P., Das, A.R., Guha, A.K., 2005. Adsorption of a model anionic dye, eosin Y, from aqueous solution by chitosan hydrobeads. 22 J. Colloid Interface Sci. 288, 30–35. doi:10.1016/j.jcis.2005.02.055. Chen, X.G., Park, H.J., 2003. Chemical characteristics of O-carboxymethyl chitosans related to the preparation conditions. Carbohydr. Polym. 53, 355–359. doi:10.1016/S0144-8617(03)00051-1. Choi, J., Chung, J., Lee, W., Kim, J.O., 2016. Phosphorous adsorption on synthesized magnetite in wastewater. J. Ind. Eng. Chem. 34, 198–203. doi:10.1016/j.jiec.2015.11.008. Cooke, G.D., Welch, E.B., Peterson, S.A., Nichols, S.A., 2005. Restoration and management of lakes and reservoirs, third edition, Taylor and Francis Group, Boca Raton, Florida. Crane, R.A., Scott, T.B., 2012. Nanoscale zero-valent iron: Future prospects for an emerging water treatment technology. J. Hazard. Mater. 211-212, 112–125. doi:10.1016/j.jhazmat.2011.11.073. Crini, G., Badot, P.M., 2008. Application of chitosan, a natural aminopolysaccharide, for dye removal from aqueous solutions by adsorption processes using batch studies: A review of recent literature. Prog. Polym. Sci. 33, 399–447. doi:10.1016/j.progpolymsci.2007.11.001. Daou, T.J., Begin-Colin, S., Grenche, J.M., Thomas, F., Derory, A., Bernhardt, P., Legar, P., Pourroy, G., 2007. Phosphate adsorption properties of magnetitebased nanoparticles. Chem. Mater. 19, 4494–4505. doi:10.1021/cm071046v. de Vicente, I., Huang, P., Andersen, F., Jensen, H.S., 2008. Phosphate adsorption by fresh and aged aluminum hydroxide. Consequences for lake restoration. 23 Environ. Sci. Technol. 42, 6650–6655. doi:10.1021/es800503s. de Vicente, I., Merino-Martos, A., Cruz-Pizarro, L., de Vicente, J., 2010. On the use of magnetic nano and microparticles for lake restoration. J. Hazard. Mater. 181, 375–381. doi:10.1016/j.jhazmat.2010.05.020. de-Bashan, L.E., Bashan, Y., 2004. Recent advances in removing phosphorus from wastewater and its future use as fertilizer (1997-2003). Water Res. 38, 4222– 4246. doi:10.1016/j.watres.2004.07.014. Dittrich, M., Gabriel, O., Rutzen, C., Koschel, R., 2011. Lake restoration by hypolimnetic Ca(OH)2 treatment: Impact on phosphorus sedimentation and release from sediment. Sci. Total Environ. 409, 1504–1515. doi:10.1016/j.scitotenv.2011.01.006. Dixon, D.R., 1984. Colour and turbidity removal with reusable magnetite particles-VII. A colloid chemistry study of the effect of inorganic ions on the efficiency of clarification. Water Res. 18, 529–534. doi:10.1016/0043-1354(84)90199-4. Egemose, S., Wauer, G., Kleeberg, A., 2009. Resuspension behaviour of aluminium treated lake sediments: effects of ageing and pH. Hydrobiologia 2, 1–15. doi:10.1007/s10750-009-9949-8. Eliaz, N., Sridh, T.M., 2008. Electrocrystallization of hydroxyapatite and its dependence on solution conditions. Cryst. Growth Des. 8, 3965–3977. doi:10.1021/cg800016h. Elwakeel, K.Z., 2009. Removal of Reactive Black 5 from aqueous solutions using magnetic chitosan resins. J. Hazard. Mater. 167, 383–392. 24 doi:10.1016/j.jhazmat.2009.01.051. Filipkowska, U., Jóźwiak, T., Szymczyk, P., 2014. Application of cross-linked chitosan for phosphate removal from aqueous solutions. Prog. Chem. Appl. Chitin Its Deriv. 19, 5–14. doi:10.15259/PCACD.19.01. Foo, K.Y., Hameed, B.H., 2010. Insights into the modeling of adsorption isotherm systems. Chem. Eng. J. 156, 2–10. doi:10.1016/j.cej.2009.09.013. Funes, A., de Vicente, J., Cruz-Pizarro, L., Álvarez-Manzaneda, I., de Vicente, I., 2016. Magnetic microparticles as a new tool for lake restoration: A microcosm experiment for evaluating the impact on phosphorus fluxes and sedimentary phosphorus pools. Water Res. 89, 366–374. doi:10.1016/j.watres.2015.11.067. Funes, A., de Vicente, J., Cruz-Pizarro, L., de Vicente, I., 2014. The influence of pH on manganese removal by magnetic microparticles in solution. Water Res. 53, 110– 122. doi:10.1016/j.watres.2014.01.029. Gibbs, M.M., Hickey, C.W., Özkundakci, D., 2011. Sustainability assessment and comparison of efficacy of four P-inactivation agents for managing internal phosphorus loads in lakes: Sediment incubations. Hydrobiologia 658, 253–275. doi:10.1007/s10750-010-0477-3. Gómez-Pastora, J., Bringas, E., Ortiz, I., 2014. Recent progress and future challenges on the use of high performance magnetic nano-adsorbents in environmental applications. Chem. Eng. J. 256, 187–204. doi:10.1016/j.cej.2014.06.119. Haghseresht, F., 2005. A revolution in phosphorus removal, Phoslock Water Solution Ltd. http://www.phoslock.com.au p. 21. 25 He, P., Davis, S.S., Illum, L., 1999. Chitosan microspheres prepared by spray drying. Int. J. Pharm. 187, 53–65. doi: 10.1016/S0378-5173(99)00125-8. Huang, H.Y., Shieh, Y.T., Shih, C.M., Twu, Y.K., 2010. Magnetic chitosan/iron (II, III) oxide nanoparticles prepared by spray-drying. Carbohydr. Polym. 81, 906–910. doi:10.1016/j.carbpol.2010.04.003. Huber, D.L., 2005. Synthesis, properties, and applications of iron nanoparticles. Small 1, 482–501. doi:10.1002/smll.200500006. Iyengar, S.J., Joy, M., Ghosh, C.K., Dey, S., Kotnala, R.K., Ghosh, S., 2014. Magnetic, X-ray and Mössbauer studies on magnetite/maghemite core–shell nanostructures fabricated through an aqueous route. RSC Adv. 4, 64919–64929. doi:10.1039/C4RA11283K. Jiang, D.S., Long, S.Y., Huang, J., Xiao, H.Y., Zhou, J.Y., 2005. Immobilization of Pycnoporus sanguineus laccase on magnetic chitosan microspheres. Biochem. Eng. J. 25, 15–23. doi:10.1016/j.bej.2005.03.007. Kalkan, N.A., Aksoy, S., Aksoy, E.A., Hasirci, N., 2012. Adsorption of reactive yellow 145 onto chitosan coated magnetite nanoparticles. J. Appl. Polym. Sci. 124, 576- 584. doi: 10.1002/app.34986. Keller, A.A., Garner, K., Miller, R.J., Lenihan, H.S., 2012. Toxicity of nano-zero valent iron to freshwater and marine organisms. PLoS One 7, 1–10. doi:10.1371/journal.pone.0043983. Kumar, S., Dutta, J., Dutta, P.K., 2009. Preparation and characterization of N- heterocyclic chitosan derivative based gels for biomedical applications. Int. J. 32 186. doi:10.1016/j.partic.2010.07.025. Zhou, Z.H., Xue, J.M., Wang, J., Chan, H.S.O., Yu, T., Shen, Z.X., 2002. NiFe2O4 nanoparticles formed in situ in silica matrix by mechanical activation. J. Appl. Phys. 91, 6015–6020. doi:10.1063/1.1462853. Zhu, X., Wang, J., Zhang, X., Chang, Y., Chen, Y., 2010. Trophic transfer of TiO2 nanoparticles from daphnia to zebrafish in a simplified freshwater food chain. Chemosphere, 79, 928-933. 33 Figures Fig. 1. SEM micrographs of (a) MCMs and (b) cross-sectioned MCMs. Fig. 2. Magnetic hysteresis curve of (a) Fe3O4 and (b) MCMs. Fig. 3. Sedimentation ratio of carbonyl Fe microparticles (closed squares), and MCMs (open circles). = sediment front determined at a constant value of transmission (5 %). = initial sample height (at time zero). Concentration: 0.72 g L-1 of carbonyl Fe particles/MCMs. pH = 7. Fig. 4. Effect of pH on P removal efficiency (bars) and on electrophoretic mobility (square symbols) of MCMs. Initial concentrations: 0.72 g MCMs L-1 and 0.01 mM P. Standard deviation is represented by vertical error bars. Fig. 5. Adsorption isotherm for Fe3O4 (open circles), MCMs (closed squares) and CMs (open triangles) at pH 7. Initial concentrations: 0.1 g Fe3O4 L-1, 0.72 g MCMs L-1, 0.62 g CMs L-1 and 0.01-0.16 mM P. Standard deviation is represented by vertical error bars. 34 Fig. 1 1a 1b 35 Fig. 2 1 2 -4000 -2000 0 2000 4000 -80 -60 -40 -20 0 20 40 60 80 Magnetization (emu g-1) Magnetic field strength (kA/m) a.- Fe3O4 b.- MCMs 3 4 36 Fig. 3 5 6 0 5 10 15 20 25 30 35 40 45 50 0.0 0.2 0.4 0.6 0.8 1.0 Carbonyl Fe H/H0 Time [min] MCMs 7 8 9 10 37 Fig. 4 11 7 8 9 0 20 40 60 80 pH P removal (%) -3 -2 -1 0 1 2 3 Electrophoretic mobility (µm cm V-1s-1 12 13 38 Fig. 5 14 0 1 2 3 4 5 0 1 2 3 4 Fe3O4 MCMs q (mg P g-1) Ce (mg L-1) CMs 15 16 17 18 19 20 21 22